Molten Al-Zn-based plated steel sheet and method for producing same

By adjusting the composition and reheating conditions of the plating layer, the crack problem of 55% Al-Zn-type plated steel plate during bending processing is solved, and the yield elongation after high bending process is achieved is achieved, and the oil resistance is maintained. Effectiveness improves the overall performance of the plated steel plate.

CN119072554APending Publication Date: 2024-12-03JFE GALVANIZING & COATING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280093284.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2022-04-08
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The 55% Al-Zn-type coated steel plate is prone to plating cracks during bending processing, resulting in poor processing properties and reduced corrosion resistance. It is easy to produce yield elongation after heat treatment, affecting moldability.

Method used

By adjusting the composition of the plating layer, it contains 40% to 70% by mass of Al and 0.5% to 3.0% by mass of Si, and controls the cooling time and temperature during the reheating process to ensure bending processability and yield after aging The elongation is less than 10%, and the precipitation of Fe3C is suppressed, and excellent moldability is formed.

Benefits of technology

It achieves excellent yield elongation after high bending processability and aging, maintains oil pot resistance, and suppresses wrinkles during processing, improving the overall performance of the plated steel plate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072554A_ABST
    Figure CN119072554A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a molten Al-Zn plated steel sheet having high bendability and excellent yield elongation and moldability after aging. In order to achieve the purpose, the present invention is a molten Al-Zn-based plated steel sheet in which a plating layer has a composition containing 40-70 mass% of Al and 0.5-3.0 mass% of Si, with the remainder comprising Zn and unavoidable impurities, and in a bending test in accordance with a plating adhesion test described in JIS G 3321 (2019), the plating layer is formed at an inner interval nt (wherein n is greater than or equal to 2). Wherein, t is the thickness of the plated steel sheet, and n is the number of plated steel sheets), the bending workability represented by the smallest nt at which cracks are not confirmed when a test piece is bent by 180 degrees and the outer surface of the bent part is observed with a 10-fold magnifier is 6 t or less, and the yield elongation (YEL) after an aging acceleration test is 10% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a molten Al-Zn based plated steel sheet having high bending workability and excellent yield elongation and formability after aging, and a method for producing the same. Background Art

[0002] Molten Al-Zn plated steel sheets, represented by 55% Al-Zn plated steel sheets, in which the plating layer contains 20% to 95% Al by mass (hereinafter sometimes referred to as "55% Al-Zn plated steel sheets"), show excellent corrosion resistance. Therefore, the demand for them has been increasing in recent years, mainly in the building materials field.

[0003] However, the 55% Al-Zn type plated steel sheet has a harder coating layer than a pure zinc coating layer, so when the plated steel sheet is bent, cracks are easily generated in the processed portion of the coating layer. Such cracks in the coating layer during processing may cause the corrosion resistance of the processed portion to deteriorate, so it is desired to improve this.

[0004] In order to improve such workability or corrosion resistance of worked parts, there is known a technique of softening a plating layer by subjecting a steel sheet after forming a plating layer to heat treatment (see, for example, Patent Documents 1 to 3).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2002-322573

[0008] Patent Document 2: Japanese Patent Application Publication No. 2003-213395

[0009] Patent Document 3: Japanese Patent Application Publication No. 2006-70326 Summary of the invention

[0010] Technical problem to be solved by the invention

[0011] Regarding the technology of heat treating the steel sheet after forming the coating layer as shown in Patent Documents 1 to 3, although the workability of the molten Al-Zn plated steel sheet can be improved to a certain extent, when low carbon steel, which is often used as a general building material, is used as the raw steel sheet, there is a problem that yield elongation is easily generated in the steel sheet due to the heat treatment.

[0012] This is presumably because, when heat treatment is applied to the steel sheet after the coating layer is formed to improve workability, a large amount of Fe3C is precipitated in the dislocations introduced by the skin pass rolling step of the continuous hot-dip galvanizing line (CGL), and the precipitated Fe3C is dissolved again in the coating and baking step of the next process, resulting in an increase in the dissolved C in the steel near the dislocations.

[0013] Here, Figure 2 The relationship between the cooling time and temperature after reheating the steel sheet with the coating layer formed thereon, and the state of the Fe3C nose (ノーズ) are shown. However, when observing the Fe3C precipitation nose of the low-carbon steel sheet, the cooling rate after coating on the continuous hot-dip galvanizing line (CGL) usually avoids the precipitation nose, so Fe3C hardly precipitates. However, in the case of heat treatment as shown in patent documents 1 to 3 to improve the bending workability of the coating, the thermal history of the steel sheet sometimes affects the precipitation nose during the heat treatment process, especially during cooling after heating. In this case, Fe3C is precipitated by the dislocation introduced in the skin pass rolling step of the CGL. It is believed that in the case of manufacturing the coated steel sheet, the precipitated Fe3C is solid-dissolved again in the coating baking step of the next step, resulting in an increase in the solid-dissolved C in the steel near the dislocation compared to the main body, and the solid-dissolved C is fixed to the dislocation due to aging, thereby generating yield elongation.

[0014] Furthermore, since the generated yield elongation causes wrinkles (tensile strain) during processing, the development of a technology capable of suppressing the yield elongation is desired.

[0015] In addition, the plated steel sheet disclosed in the present invention is often used as a coated steel sheet when used as a building material. In this case, in order to suppress the above-mentioned yield elongation, it is known to give strain to the steel sheet by skin-pass rolling or tension leveling machine in the coating line (CCL) as the final step. However, in such a method, since the yield point (YP) of the steel sheet is lowered, it becomes the main reason for the deterioration of the pitting resistance (oil pot resistance) of the steel sheet (reduction of oil pot resistance). Therefore, in order to suppress the yield elongation of the low-carbon steel sheet while maintaining the oil pot resistance well, other methods are needed.

[0016] Furthermore, the yield elongation of the molten Al-Zn-based plated steel sheet mentioned above tends to deteriorate particularly after a certain period of time because it takes time for the solid solution C near the dislocation to diffuse into the dislocation. Therefore, a technology that can improve the yield elongation after aging is also desired.

[0017] In view of the above circumstances, an object of the present invention is to provide a hot-dip Al-Zn-based plated steel sheet having high bending workability and excellent yield elongation and formability after aging, and a method for producing the same.

[0018] Technical means for solving technical problems

[0019] In order to solve the above-mentioned problems, the inventors of the present application studied molten Al-Zn plated steel sheets (which have a coating layer having the following composition: containing 40 mass % to 70 mass % of Al and 0.5 mass % to 3.0 mass % of Si, with the remainder consisting of Zn and unavoidable impurities). As a result, it was found that by making improvements in the following manner, namely, optimizing the heat treatment conditions for improving the bending workability of the coating and suppressing the yield elongation (YEL) after the aging acceleration test to less than 10%, it is possible to maintain good anti-oil pot effect and suppress wrinkles during processing, thereby achieving excellent formability.

[0020] The present invention has been accomplished based on the above findings, and the gist of the present invention is as follows.

[0021] 1. A molten Al-Zn plated steel sheet, characterized in that:

[0022] The plating layer has a composition containing 40 mass % to 70 mass % of Al and 0.5 mass % to 3.0 mass % of Si, with the remainder being Zn and inevitable impurities.

[0023] In the bending test of the adhesion test of the plating described in JIS G 3321 (2019), the test piece is bent 180° with an inner spacing nt, and the bending workability represented by the minimum nt at which no cracks are confirmed when the outer surface of the bent portion is observed using a 10x magnifying glass is less than 6t, and the yield elongation (YEL) after the aging acceleration test is less than 10%, wherein t is the thickness of the plated steel sheet, and n is the number of plated steel sheets.

[0024] 2. The molten Al-Zn-based plated steel sheet according to item 1, wherein the Al primary crystals in the dendrite phase in the plated layer have a Vickers hardness of 120 HV 0.01 the following.

[0025] 3. A method for producing a molten Al-Zn-based plated steel sheet, characterized in that:

[0026] After forming a coating layer on a base steel sheet using a coating bath, when the steel sheet having the coating layer formed thereon is reheated, the highest temperature reached by the steel sheet is set to T (° C.), and the cooling time from T° C. to 150° C. is set to x (hr), the following equations (1) and (2) are satisfied:

[0027] The plating bath has a composition comprising 40 mass % to 70 mass % of Al and 0.5 mass % to 3.0 mass % of Si, and the remainder is composed of Zn and unavoidable impurities,

[0028] 150≤T≤300··· (1)

[0029] 0.5≤x≤1000 / (T+273) ··· (2).

[0030] Effects of the Invention

[0031] According to the present invention, it is possible to provide a hot-dip Al-Zn-based plated steel sheet having high bending workability and excellent yield elongation and formability after aging, and a method for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] [ Figure 1 ] is a diagram schematically showing a state where a molten Al-Zn-based plated steel sheet is subjected to 180° bending processing.

[0033] [ Figure 2 ] is a diagram showing the relationship between the cooling time and temperature after reheating of a steel sheet having a coating layer formed thereon, and the state of the Fe3C nose.

[0034] [ Figure 3 ] is a diagram schematically showing a shape formed for the moldability evaluation of the embodiment. DETAILED DESCRIPTION

[0035] <Molten Al-Zn type plated steel sheet>

[0036] The molten Al-Zn plated steel sheet of the present invention has a composition in which the plated layer contains 40 to 70 mass % of Al and 0.5 to 3.0 mass % of Si, and the remainder is Zn and unavoidable impurities.

[0037] (Composition of the plating layer)

[0038] The coating layer has the following composition: 40 mass % to 70 mass % Al and 0.5 mass % to 3.0 mass % Si, and the remainder is composed of Zn and inevitable impurities. Since the coating layer of the molten Al-Zn type plated steel sheet has the above composition, a dendrite phase and an interdendritic phase surrounding the dendrite phase in a grid shape can be formed in the coating layer, thereby improving the corrosion resistance.

[0039] As for the Al content in the coating layer, from the perspective of the balance between corrosion resistance and operation, it is set to 40% to 70% by mass, preferably 50% to 60% by mass. If the Al content of the main layer of the coating layer is at least 40% by mass, the dendrite solidification of Al can be fully caused. Thus, the main layer is mainly composed of a portion (dendritic phase of α-Al phase) in which Zn is supersaturated and Al undergoes dendrite solidification and a portion (interdendritic phase) in the remaining dendrite gap, and a structure with excellent corrosion resistance in which the dendrite phase is stacked in the film thickness direction of the coating layer can be achieved. In addition, the more the dendritic phase of the α-Al phase is stacked, the more complicated the corrosion path becomes, and the more difficult it is for corrosion to reach the base steel plate, so the corrosion resistance is improved. On the other hand, if the Al content in the coating layer exceeds 70% by mass, the content of Zn that has a sacrificial anti-corrosion effect on Fe decreases, and the corrosion resistance deteriorates. Therefore, the Al content in the coating layer is set to 70% or less by mass. In addition, if the Al content in the plating layer is 60% by mass or less, the amount of plating adhesion becomes less, and even if the base steel sheet is easily exposed, it has a sacrificial corrosion protection effect on Fe, and sufficient corrosion resistance can be obtained. Therefore, the Al content of the plating main layer is preferably set to 70% by mass or less.

[0040] The Si in the coating layer is added to the coating bath for the purpose of suppressing the growth of the interface alloy layer generated at the interface with the base steel sheet and for the purpose of improving corrosion resistance or workability, and is necessarily contained in the coating layer. In the case of the molten Al-Zn type plated steel sheet used in the molten Al-Zn type plated steel sheet of the present invention, if the coating bath contains Si and the molten coating treatment is performed, while the base steel sheet is immersed in the coating bath, the Fe on the surface of the steel sheet reacts with the Al or Si in the bath to form an alloy composed of Fe-Al and / or Fe-Al-Si type compounds. The growth of the interface alloy layer can be suppressed by the formation of the Fe-Al-Si type interface alloy layer. Moreover, when the Si content in the coating layer is 0.5% by mass or more, the growth of the interface alloy layer can be fully suppressed. On the other hand, when the Si content in the coating layer exceeds 3.0% by mass, in the coating layer, the workability is reduced, and the Si phase that becomes the cathode part becomes easy to precipitate. Therefore, the Si content in the plating layer is set to 0.5 mass % to 3.0 mass %.

[0041] In addition, the plating layer contains Zn as the main component of the plating layer. Since the plating layer contains Zn, a sacrificial anti-corrosion effect can be obtained, and the improvement of corrosion resistance can be sought. In addition, when the content of Zn is 80% by mass or less, the Al content can be ensured, and the corrosion resistance obtained by the above-mentioned dendrite phase and interdendritic phase can be achieved, which is preferred in this regard.

[0042] Furthermore, the plating layer may contain 5 mass % or less of any additional component in addition to the above-mentioned Al, Si and Zn.

[0043] Here, the optional additive components can be appropriately selected according to the performance required for the coating layer, and for example, alkaline earth metals such as Ca or Mg, or additive components such as Mn, V, Cr, Mo, Ti, Sr, Ni, Co, Sb, and B can be cited.

[0044] These optional additives can further improve the corrosion resistance, but may also reduce the workability of the coating layer and deteriorate the ultimate elongation of the molten Al-Zn-based plated steel sheet. Therefore, the content of the optional additives is preferably 5 mass % or less.

[0045] The plating layer may contain Mg and / or Ca. When the plating layer corrodes, the corrosion product contains Mg and / or Ca, the stability of the corrosion product is improved, and the corrosion progress is slowed down, resulting in an effect of improved corrosion resistance. The total content of Ca and / or Mg is 5% by mass or less, and is not particularly limited, preferably 0.01% by mass to 5% by mass. The reason is that by setting the content to 0.01% by mass or more, a sufficient corrosion delay effect can be obtained. On the other hand, by setting the content to 5% by mass or less, the effect will not be saturated, the increase in manufacturing costs can be suppressed, and the composition management of the plating bath can be easily performed.

[0046] In addition, the plating layer preferably contains at least Mg. The reason is that the plating layer contains Mg, which can generate Mg2Si together with Si, thereby obtaining a corrosion delay effect. Here, the content of Mg in the plating layer is preferably 0.01 mass% to 5 mass%, and more preferably 2 mass% to 4.9 mass%.

[0047] Furthermore, similar to the alkaline earth metals of Ca or Mg, the plating layer has the effect of improving the stability of corrosion products and delaying the progress of corrosion. Therefore, the plating layer may also contain a total of less than 5 mass%, preferably 0.01 mass% to 5 mass%, of one or more selected from Mn, V, Cr, Mo, Ti, Sr, Ni, Co, Sb and B.

[0048] In addition, the coating layer includes: base steel plate components mixed into the coating due to the reaction between the coating bath and the base steel plate during the coating process, or inevitable impurities contained in the ingot used when the coating bath is built, and some inevitable impurities dissolved from the bath machine. As a base steel plate component mixed into the coating, it sometimes contains a few % of Fe. As the types of inevitable impurities in the coating bath, for example, as base steel plate components, Fe, Mn, P, S, C, Nb, Ti, B, etc. can be listed. In addition, as impurities in the ingot, Fe, Pb, Sb, Cd, As, Ga, V, etc. can be listed. Further, as impurities from the machine in the bath, Cr, Ni, W, Co, etc. can be listed. In addition, with regard to the Fe in the coating layer, it is impossible to distinguish and quantify the Fe mixed from the base steel plate and the Fe present in the coating bath. The total content of the inevitable impurities is not particularly limited, but from the viewpoint of maintaining the corrosion resistance and uniform solubility of the plating, the total content of the inevitable impurities other than Fe is preferably 1 mass % or less.

[0049] In addition, there is no particular limitation on the method for forming the coating layer on the base steel plate, and a general continuous molten-coating device can be used. For example, the base steel plate is heated to a specified temperature in an annealing furnace maintained in a reducing atmosphere, and the rolling oil attached to the surface of the steel plate is removed while annealing, and after the oxide film is reduced and removed, the lower end passes through a furnace nose immersed in a coating bath and is immersed in a molten galvanizing bath containing a specified concentration of Al and Zn. Then, the steel plate immersed in the coating bath is pulled to the top of the coating bath via a sinking roll, and the coating adhesion amount is adjusted by spraying pressurized gas from a gas wiping nozzle arranged on the coating bath toward the surface of the steel plate, and then cooled by a cooling device, thereby forming a coating layer.

[0050] In addition, the coating layer has a dendrite phase and an interdendrite phase in its structure, and the Vickers hardness of the Al primary crystals in the dendrite phase is preferably 120 HV. 0.01 By reducing the Vickers hardness of the Al primary crystals of the dendrite phase to 120 HV 0.01 The bending workability of the plated steel sheet described below can be further improved. From the same viewpoint, the Vickers hardness of the Al primary crystals in the dendrite phase in the plated layer is more preferably 110 HV 0.01 Below, more preferably 100HV 0.01 On the other hand, from the viewpoint of improving the scratch resistance of the surface of the coating layer, the Vickers hardness of the Al primary crystals in the dendrite phase is preferably 10 HV 0.01 above.

[0051] In addition, regarding the Vickers hardness, under an indentation load of 10 g (HV 0.01 ) was carried out under the

[0052] Furthermore, the coating weight of the plating layer is not particularly limited, but from the viewpoint of achieving both corrosion resistance and bending workability, the coating weight on one side is preferably 30 g / m 2 ~90g / m 2 , more preferably 40g / m 2 ~80g / m 2 .

[0053] Furthermore, the plating layer has an interface alloy layer present at an interface between the plating layer and the base steel sheet.

[0054] The interface alloy layer is a Fe-Al and / or Fe-Al-Si compound that is inevitably generated by the alloying reaction between the Fe on the surface of the steel plate and the Al or Si in the bath. Since the interface alloy layer is hard and brittle, if it grows thicker, it will become the starting point of cracks during processing, so it is preferably as thin as possible. Therefore, it is preferred that the thickness of the interface alloy layer be set to less than 1 μm.

[0055] (Bending properties)

[0056] Here, in the molten Al-Zn type plated steel sheet of the present invention, in the bending test of the adhesion test of the plating described in JIS G 3321 (2019), the test piece is bent 180° with an inner spacing nt, and the bending workability represented by the minimum nt in which no crack is confirmed when the outer surface of the bent portion is observed with a 10x magnifying glass is 6t or less. By making the bending workability 6t or less, excellent bending workability can be achieved, and then corrosion resistance after processing can be achieved.

[0057] From the same viewpoint, the bending workability of the molten Al—Zn-based plated steel sheet of the present invention is preferably 5 t or less, and more preferably 4 t or less.

[0058] In addition, the bending test for obtaining the bending workability is a bending test according to the adhesion test of the plating described in JIS G 3321 (2019), such as Figure 1 As shown, t of the inner interval nt is the plate thickness of the plated steel plate, and n is the number of plated steel plates, for example, 2t when two steel plates are sandwiched, and 3t when three steel plates are sandwiched.

[0059] The entire surface of the bent portion of the test piece was observed with a 10x magnifying glass to confirm the presence or absence of cracks. For example, in the bending test, if there were no cracks until 3t, and cracks were confirmed when the bending test was performed at 2t, the bending workability of the steel plate was 3t.

[0060] (YEL, YP after aging test)

[0061] Furthermore, the hot-dip Al-Zn-based plated steel sheet of the present invention is characterized in that, while satisfying the above-mentioned bending workability (6 t or less), the yield elongation (YEL) after an aging accelerated test is 10% or less.

[0062] By suppressing the YEL after the accelerated aging test to less than 10%, the oil pot effect resistance can be well maintained, and wrinkles during processing can also be suppressed, so that excellent moldability can be achieved. In addition, since the YEL after accelerated aging is specified, there is no need to consider the subsequent deterioration of YEL due to aging, and the yield elongation after aging is also excellent. From the same point of view, the YEL after the accelerated aging test is preferably less than 9.0%, more preferably less than 8.5%, and even more preferably less than 8.0%.

[0063] Here, the YEL can be measured by a tensile test. In the present invention, a No. 5 test piece of JIS Z 2201 is collected from a molten Al-Zn type plated steel sheet, and the strain rate is 10 -3 The tensile test was carried out under the condition of s.

[0064] In the present invention, as the accelerated aging test, an accelerated aging treatment of maintaining at 100° C. for 3600 seconds is performed.

[0065] That is, the YEL after the accelerated aging test can be measured by collecting a test piece from a molten Al-Zn-based plated steel sheet, subjecting the test piece to an accelerated aging treatment at 100° C. for 3600 seconds, and then subjecting the test piece to a tensile test.

[0066] In addition, regarding the molten Al-Zn type plated steel sheet of the present invention, there is no particular limitation on the method of suppressing the YEL after the aging acceleration test to be less than 10% and the method of maintaining the above-mentioned bending workability to be less than 6T. For example, there can be cited a method of controlling the composition of the coating layer, the temperature conditions when forming the coating layer, the temperature conditions when reheating after forming the coating layer, etc.

[0067] For example, in the present invention, as described later, the temperature conditions during reheating after forming the plating layer are controlled to control the YEL and the bending workability after the accelerated aging test.

[0068] In addition, the yield point (YP) of the molten Al-Zn based plated steel sheet of the present invention is preferably 400 N / mm 2 More than, more preferably 450N / mm 2 The reason is that even when YP is less than 400N / mm 2 Even when YEL is good, the anti-oil pot effect will decrease, which may lead to poor moldability.

[0069] In addition, in the hot-dip Al-Zn type plated steel sheet of the present invention, a coating film may be formed directly on the plated layer or via an intermediate layer depending on the required performance.

[0070] In addition, there is no particular limitation on the method for forming the coating film, and it can be appropriately selected according to the required performance. For example, a forming method such as roller coating, curtain coating, spray coating, etc. can be cited. After the coating containing the organic resin is applied, it can be heated and dried by means such as hot air drying, infrared heating, induction heating, etc. to form a coating film.

[0071] The intermediate layer is not particularly limited as long as it is a layer formed between the plated film of the hot-dip plated steel sheet and the coating film.

[0072] <Method for producing molten Al-Zn plated steel sheet>

[0073] The method for producing a molten Al-Zn type plated steel sheet of the present invention (hereinafter sometimes referred to as "the production method of the present invention") is characterized in that after forming a plated layer on a base steel sheet using a plating bath (having a composition comprising 40 mass % to 70 mass % of Al and 0.5 mass % to 3.0 mass % of Si, with the remainder consisting of Zn and inevitable impurities), when the maximum temperature reached by the steel sheet when the steel sheet having the plated layer formed thereon is reheated is set to T (°C) and the residence time at 150°C to T°C is set to x (hr), the following formulas (1) and (2) are satisfied:

[0074] 150≤T≤300··· (1)

[0075] 0.5≤x≤1000 / (T+273) ··· (2).

[0076] In the past, in order to suppress the YEL of molten Al-Zn-type plated steel sheets, there is a known method of applying strain to the steel sheets through skin smooth rolling or tension leveling machines on a coating production line. However, when these methods are used, the yield point (YP) of the steel sheets is lowered, which becomes the main reason for the deterioration of the anti-oil pot effect of the steel sheets.

[0077] Therefore, in the manufacturing method of the present invention, regarding the temperature conditions when reheating the steel plate formed with the above-mentioned coating layer, by specifying the temperature range of the highest temperature T reached by the steel plate, and at the same time specifying the range of the residence time x of the steel plate above 150°C, that is, satisfying equations (1) and (2), in addition to achieving excellent bending workability, it is also possible to maintain good anti-oil pot effect and suppress the YEL of the molten Al-Zn type plated steel plate after the aging acceleration test.

[0078] In addition, in the manufacturing method of the hot-dip Al-Zn type plated steel sheet of the present invention, there is no particular limitation, but from the viewpoint of manufacturing efficiency or quality stability, a continuous hot-dip coating facility is generally used.

[0079] In addition, there is no particular limitation on the type of base steel sheet used in the manufacturing method of the present invention. For example, a hot-rolled steel sheet or strip that has been pickled to remove scale (pickling to remove scale) or a cold-rolled steel sheet or strip obtained by cold rolling them can be used. However, from the viewpoint of more significantly obtaining the effect of suppressing YEL after the aging acceleration test according to the present invention, it is preferable to use low-carbon steel that is also preferred in terms of cost.

[0080] Furthermore, even as a component in steel, it is not particularly limited in the present invention, for example, a material with C: 0.01 to 0.10 mass % can be used. However, steel plates with C: less than 0.01% are not excluded in the present invention. In addition, steel plates containing N, S, O, B, V, Nb, Ti, Cu, Mo, Cr, Co, Ni, Ca, Sr, In, Sn, Sb, etc. as trace additive elements in addition to C, Al, Si, Mn, and P also fall within the scope of the present invention.

[0081] In the production method of the present invention, the plating bath has a composition containing 40 mass % to 70 mass % of Al and 0.5 mass % to 3.0 mass % of Si, with the remainder being Zn and unavoidable impurities.

[0082] Thereby, a hot-dip Al-Zn-based plated steel sheet having a desired composition can be obtained. In addition, the type, content, and function of each element contained in the coating bath are described in the hot-dip Al-Zn-based plated steel sheet of the present invention.

[0083] In addition, the molten Al-Zn plated steel sheet obtained by the manufacturing method of the present invention has substantially the same composition as the coating bath as a whole. Therefore, the composition of the coating layer of the molten Al-Zn plated steel sheet can be controlled by adjusting the coating bath composition.

[0084] In the manufacturing method of the present invention, when the steel sheet having the coating layer formed thereon is reheated, the maximum temperature T reaches satisfies the following formula (1).

[0085] 150≤T≤300··· (1)

[0086] In formula (1), the range of the maximum temperature T when the steel sheet with the coating layer is reheated is specified. The reason for setting the maximum temperature T to be 150°C or higher is that if it is not higher than this temperature, the coating layer will not be sufficiently softened, so the bending workability of the molten Al-Zn type plated steel sheet is reduced. On the other hand, the reason for setting the maximum temperature T to be 300°C or lower is that at a temperature higher than this, the thickness of the interface alloy layer generated at the interface between the coating and the steel sheet becomes thick, resulting in a reduction in the bending workability.

[0087] In the manufacturing method of the present invention, when the steel sheet having the coating layer formed thereon is reheated, the cooling time x from T°C to 150°C satisfies the following formula (2).

[0088] 0.5≤x≤1000 / (T+273) ··· (2)

[0089] By specifying the cooling time x of the highest reaching temperature T℃ to 150℃ as shown in formula (2), the precipitation nose of Fe3C (the condition where Fe3C is easily precipitated) can be avoided, so the amount of solid solution C can be reduced, and the yield elongation and the yield elongation after the aging acceleration test can be suppressed. In addition, when the residence time x is less than 0.5hr, the coating layer cannot be fully softened, so that good bending workability cannot be ensured. On the other hand, if the cooling time x exceeds 1000 / (T+273), the nose may be precipitated by Fe3C, so the amount of solid solution C cannot be reduced, so that the yield elongation cannot be suppressed.

[0090] In addition, in the manufacturing method of the present invention, for the steel plate formed with the above-mentioned coating layer, since there is no need to apply strain to the steel plate through surface smooth rolling or tension leveling machine on the coating production line, it will not lead to deterioration of formability such as anti-oil pot effect caused by a decrease in YP.

[0091] Here, Figure 2The relationship between the cooling time and the temperature when the steel plate having the coating layer is reheated, and the state of the Fe3C precipitation nose are shown. As described above, in order to suppress the yield elongation caused by aging during the cooling after reheating, it is necessary to avoid the Fe3C precipitation nose as much as possible when cooling from the maximum temperature T°C. Therefore, in the manufacturing method of the present invention, by controlling the cooling time from the maximum temperature T°C to 150°C, the Fe3C precipitation nose during cooling can be avoided, thereby achieving the purpose. Figure 2 It is clear that in order to avoid the precipitation of Fe3C in the nose, the cooling time needs to be shortened when T is high. The upper limit of the cooling time is represented by 1000 / (T+273). In addition, as mentioned above, the lower limit is determined to ensure the processability of the coating. Figure 2 The "cooling satisfying the formula (2)" shown in FIG. 1 shows an example of a cooling method from T°C to 150°C. The cooling curve in the figure is only an example, and the cooling rate is not specified in the present invention.

[0092] In the manufacturing method of the present invention, as described above, as long as the composition of the coating bath and the conditions for reheating the steel sheet having the coating layer formed thereon are satisfied, other conditions are not particularly limited and may be the same as those of the known molten Al-Zn based plated steel sheet.

[0093] Example

[0094] Hereinafter, the present invention will be described with reference to specific examples and comparative examples, but the present invention is not limited to the following examples.

[0095] <Samples 1 to 9 of molten Al-Zn-based plated steel sheets>

[0096] A cold-rolled steel sheet having a thickness of 0.40 mm produced by a common method was used as a base steel sheet, and was subjected to annealing treatment, plating treatment, and skin pass rolling treatment by a continuous hot-dip plating equipment.

[0097] Next, the coil was heat treated in a batch heating furnace under the conditions shown in Table 1. In addition, the temperature of the steel plate was measured by a thermocouple attached to the steel plate. Furthermore, the coil was chemically converted and coated with a primer and a topcoat in the continuous coating line. In addition, for some samples, an elongation of 0.1% was given to the steel plate by a tension leveler after coating.

[0098] Thus, samples 1 to 9 shown in Table 1 were prepared.

[0099] In addition, the thickness of the interface alloy layer of each sample was measured by cross-sectional observation (X2000) of the plated layer using SEM.

[0100] In addition, regarding the Vickers hardness of the dendrite phase in the plating layer of each sample, each sample was embedded in a room temperature dried resin and ground, and the dendrite phase of the plating layer was selected from the cross section, and the Vickers hardness of the selected dendrite phase was measured using a microhardness tester (manufactured by Shimadzu Corporation, Shimadzu microhardness tester HMV-G21). The measurement method was carried out using a method in accordance with JIS Z 2244, and was implemented with a press load of 10 gf.

[0101] <Evaluation>

[0102] The following evaluations were performed on the melt-coated Al-Zn-based plated steel sheets of the respective samples obtained as described above. The evaluation results are shown in Table 1.

[0103] (1) Bending resistance

[0104] The molten Al-Zn type plated steel sheets of each sample were subjected to a bending test according to the coating adhesion test described in JIS G 3321 (2019). The steel sheets were bent 180 degrees with a width of 50 mm, and five locations of the cross section of the bent portion within a width of 30 mm except for 10 mm at both ends were observed through a 10x magnifying glass to measure the minimum nt (where t is the thickness of the plated steel sheet, and n is the number of plated steel sheets) at which no cracks were confirmed.

[0105] Then, the obtained nt was evaluated according to the following criteria.

[0106] ○: 6t or less

[0107] ×: 7t or more

[0108] (2) YEL after time-acceleration test

[0109] A No. 5 test piece of JIS Z 2201 was collected from the molten Al-Zn type plated steel sheet of each sample and subjected to a strain of 10 -3 In addition, from the time of collecting each test piece to the time of tensile testing, an aging acceleration test was performed at 100°C for 3600 seconds, and then a tensile test according to JIS Z 2241 was performed to measure the yield point elongation.

[0110] The tensile test was performed three times each in the L and C directions of the steel plate (N=3), and the average values ​​thereof were taken.

[0111] (3) Formability (wrinkle or no wrinkle, oil pot resistance)

[0112] The molten Al-Zn-based plated steel sheets of each sample were formed into Figure 3 After the shapes shown were obtained, the presence or absence of wrinkles and the generation of pits at the flat end portions were visually checked.

[0113] Regarding the evaluation, the sample with no wrinkles or pits was rated as ○, and the sample with wrinkles or pits was rated as ×.

[0114]

[0115] As can be seen from the results in Table 1, each sample of the present invention is well-balanced and excellent in any of the bending resistance, YEL after accelerated aging, and formability (presence of wrinkles, anti-oil pot effect) compared with each sample of the comparative example.

[0116] (Industrial Applicability)

[0117] According to the present invention, it is possible to provide a hot-dip Al-Zn-based plated steel sheet having high bending workability and excellent yield elongation and formability after aging, and a method for producing the same.

Claims

1. A molten Al-Zn plated steel sheet, characterized in that: The plating layer has a composition containing 40 mass % to 70 mass % of Al and 0.5 mass % to 3.0 mass % of Si, with the remainder being Zn and inevitable impurities. In the bending test of the adhesion test of the plating described in JIS G 3321 (2019), the test piece is bent 180° with an inner spacing nt, and the bending workability represented by the minimum nt at which no cracks are confirmed when the outer surface of the bent portion is observed using a 10x magnifying glass is less than 6t, and the yield elongation (YEL) after the aging acceleration test is less than 10%, wherein t is the thickness of the plated steel sheet, and n is the number of plated steel sheets.

2. The molten Al-Zn based plated steel sheet according to claim 1, characterized in that: The Vickers hardness of the Al primary crystals in the dendrite phase in the coating layer is 120 HV 0.01 the following.

3. A method for producing a molten Al-Zn-based plated steel sheet, characterized in that: After forming a coating layer on a base steel sheet using a coating bath, when the steel sheet having the coating layer formed thereon is reheated, the highest temperature reached by the steel sheet is set to T (° C.), and the cooling time from T° C. to 150° C. is set to x (hr), the following equations (1) and (2) are satisfied: The plating bath has a composition comprising 40 mass % to 70 mass % of Al and 0.5 mass % to 3.0 mass % of Si, and the remainder is composed of Zn and unavoidable impurities, 150≤T≤300··· (1) 0.5≤x≤1000 / (T+273) ··· (2).