Silicon-coated antioxidant iron, silicon-coated antioxidant nickel and preparation method thereof
By evaporating silicon, silicon-oxygen-iron or silicon-oxygen-nickel hybrid layer, the problem of metal surface oxidation under high temperature conditions is solved, and the process is simplified and the high-cost antioxidant effect is achieved. It is suitable for iron and nickel surface.
Patent Information
- Application Number
- CN202380035572.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-28
- Filing Date
- 2023-04-28
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to effectively prevent the oxidation of the metal surface under high temperature conditions, resulting in a reduction in durability, and the commonly used coating methods are complex and costly.
By evaporating silicon, silicon-oxygen-iron or silicon-oxygen-nickel mixed layer is formed to form an antioxidant film. A single-step process is carried out under argon atmosphere at room temperature to 350°C, simplifying the process and improving the preparation efficiency .
The oxidation of iron and nickel surfaces is effectively prevented within the temperature range of 200°C to 350°C, keep the electrical characteristics unchanged, and provides an antioxidant film with high temperature oxidation resistance and economical value. The preparation method is simple and cheap.
Smart Images

Figure CN119072556A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to silicon-coated anti-oxidation iron, silicon-coated anti-oxidation nickel and a preparation method thereof, and more particularly, to surface-coated silicon (Si) anti-oxidation iron having an anti-oxidation property and maintaining electrical properties by forming a silicon (Si)-oxygen (O)-iron (Fe) mixed layer protective film by evaporating silicon (Si), and surface-coated silicon (Si) anti-oxidation nickel having an anti-oxidation property and maintaining electrical properties by forming a silicon (Si)-oxygen (O)-nickel (Ni) mixed layer protective film by evaporating silicon (Si), and a preparation method thereof. Background Art
[0002] Generally, metal materials are oxidized and corroded due to interaction with the surrounding environment, resulting in reduced durability of the metal itself. Currently, methods for preventing metal corrosion include preparing chemically stable alloys by adding other elements to the metal itself and treating the metal surface by coating or the like.
[0003] The above-mentioned surface coating method can selectively use coating materials according to the characteristics, application and surrounding environment of the metal. Although it has the advantage of improving corrosion resistance, it has the disadvantage of limited use under high temperature conditions.
[0004] Therefore, in order to solve the above-mentioned problems, a metal surface coating method which has a simple process and can solve the oxidation problem is required. Summary of the invention
[0005] Technical issues
[0006] The present invention is proposed to solve the above-mentioned problems. The purpose of the present invention is to provide a method for preparing the following anti-oxidation iron film, that is, not only can it prevent oxidation by forming a silicon (Si)-oxygen (O)-iron (Fe) protective layer by evaporating silicon (Si), but also it can stably prevent oxidation even under high temperature conditions.
[0007] The present invention is proposed to solve the above-mentioned problems. Another object of the present invention is to provide a method for an anti-oxidation nickel film, which can not only prevent oxidation by forming a silicon (Si)-oxygen (O)-nickel (Ni) protective layer by evaporating silicon (Si), but also can stably prevent oxidation even under high temperature conditions.
[0008] The technical problems to be solved by the present invention are not limited to the above-mentioned technical problems. Ordinary technicians in the technical field to which the present invention belongs can clearly understand other technical problems not mentioned through the following records.
[0009] Technical Solution
[0010] The invention relates to silicon-coated anti-oxidation iron, which forms a silicon (Si)-oxygen (O)-iron (Fe) mixed layer on the silicon-coated anti-oxidation iron by evaporating silicon (Si).
[0011] Furthermore, the electrical resistance of the silicon-coated anti-oxidation iron is similar to that of iron without the silicon vapor deposition.
[0012] Furthermore, the silicon-coated anti-oxidation iron is in the form of a film, foil or block.
[0013] Furthermore, when the silicon-coated anti-oxidation iron is in the form of a film, foil or block, it can be prevented from being oxidized even when heated at a temperature of 200° C. to 350° C. for 20 minutes to 40 minutes.
[0014] Moreover, the surface resistance of the silicon-coated anti-oxidation iron is 9.2×10 -4 Ω / □ to 9.6×10 -4 Ω / □.
[0015] Furthermore, the silicon-coated anti-oxidation iron comprises: an iron layer 10; an iron oxide (Fe3O4) layer 20 formed on the upper end of the iron layer 10; a ferrosilicon alloy layer 30 formed by a mixture of silicon (Si)-oxygen (O)-iron (Fe) on the upper end of the iron oxide layer 20; and a silicon (Si)-oxygen (O) mixed layer 40 formed on the upper end of the ferrosilicon alloy layer 30.
[0016] Furthermore, the thickness of the iron oxide (Fe3O4) layer 20 is 3 nm to 7 nm.
[0017] Furthermore, the thickness of the ferrosilicon alloy layer 30 formed by the mixture of silicon (Si)-oxygen (O)-iron (Fe) is 0.8 nm to 1.2 nm.
[0018] Furthermore, the thickness of the (Si)-oxygen (O) mixed layer 40 is 5 nm to 30 nm.
[0019] The invention relates to a method for preparing silicon-coated anti-oxidation iron, in which silicon (Si) is evaporated onto iron (Fe) through a single-step sputtering process.
[0020] Furthermore, the above-mentioned sputtering is performed under an argon atmosphere.
[0021] Furthermore, the sputtering is performed at a temperature ranging from room temperature to 350° C. for 1 minute to 5 minutes.
[0022] The present invention relates to silicon-coated anti-oxidation nickel, on which a silicon-nickel alloy layer 200 is formed. The silicon-nickel alloy layer 200 is a silicon (Si)-oxygen (O)-nickel (Ni) mixed layer formed by evaporating silicon (Si).
[0023] Furthermore, the electrical resistance of the silicon-coated anti-oxidation nickel is similar to that of nickel without the silicon vapor deposition.
[0024] Furthermore, the silicon-coated anti-oxidation nickel is a single crystal film, a polycrystalline film, a foil or a block.
[0025] Furthermore, when the silicon-coated anti-oxidation nickel is a single crystal thin film, it can be prevented from being oxidized even when heated at a temperature of 300° C. to 500° C. for 20 minutes to 50 minutes.
[0026] Furthermore, when the silicon-coated oxidation-resistant nickel is in the form of a polycrystalline thin film, foil or block, it can be prevented from being oxidized even when heated at a temperature of 300° C. to 400° C.
[0027] Moreover, the surface resistance of the silicon-coated anti-oxidation nickel is 6.2×10 -4 Ω / □ to 6.8×10 -4 Ω / □.
[0028] Furthermore, the silicon-coated anti-oxidation nickel includes: a nickel layer 100; a silicon-nickel alloy layer 200, formed by a mixture of silicon (Si)-oxygen (O)-nickel (Ni) on the upper end of the above-mentioned nickel layer 100; a first silicon (Si)-oxygen (O) mixed layer 300, formed on the upper end of the above-mentioned silicon-nickel alloy layer 200; and a second silicon (Si)-oxygen (O) mixed layer 400, formed on the upper end of the above-mentioned first silicon (Si)-oxygen (O) mixed layer 300.
[0029] Furthermore, the thickness of the silicon-nickel alloy layer 200 is 0.8 nm to 1.2 nm.
[0030] Furthermore, the thickness of the silicon (Si)-oxygen (O) mixed layer including the first silicon (Si)-oxygen (O) mixed layer 300 and the second silicon (Si)-oxygen (O) mixed layer 400 is 5 nm to 30 nm.
[0031] In the method for preparing silicon-coated anti-oxidation nickel of the present invention, nickel (Ni) is deposited on iron (Fe) by a single-step sputtering process.
[0032] Furthermore, the above-mentioned sputtering is performed under an argon atmosphere.
[0033] Furthermore, the sputtering is performed at a temperature ranging from room temperature to 350° C. for 1 minute to 5 minutes.
[0034] Effects of the Invention
[0035] According to the above technical scheme, the present invention can prepare antioxidant iron only by evaporating silicon (Si), thereby not only simplifying the process and improving the preparation efficiency, but also using iron (Fe) and silicon (Si) to provide antioxidant iron with high economic value.
[0036] Furthermore, the present invention can provide iron (Fe) having oxidation resistance and maintaining electrical properties by forming a silicon (Si)-oxygen (O)-iron (Fe) protective film by evaporating silicon (Si) and a preparation method thereof.
[0037] Furthermore, the present invention can provide an antioxidant iron which has a very simple preparation method, is low in cost and can be used semi-permanently at room temperature.
[0038] Furthermore, the present invention can provide antioxidant iron having greatly improved antioxidant properties under high temperature conditions.
[0039] Furthermore, the present invention only requires the evaporation of silicon (Si) to prepare oxidation-resistant nickel, thereby not only simplifying the process and improving the preparation efficiency, but also providing oxidation-resistant nickel with high economic value by using nickel (Ni) and silicon (Si).
[0040] Furthermore, the present invention can provide nickel (Ni) having oxidation resistance and maintaining electrical properties by forming a silicon (Si)-oxygen (O)-nickel (Ni) protective film by evaporating silicon (Si) and a preparation method thereof.
[0041] Furthermore, the present invention can provide oxidation-resistant nickel which has a very simple preparation method, is low in cost and can be used semi-permanently at room temperature.
[0042] Furthermore, the present invention can provide oxidation-resistant nickel having greatly improved oxidation resistance under high temperature conditions.
[0043] The effects of the present invention are not limited to the above effects, and a person skilled in the art can clearly understand other effects not mentioned through the description of the scope of protection claimed in the invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 These are photos of a common iron plate and the silicon (Si) coated iron plate of the present invention before and after heat treatment.
[0045] Figure 2 The graph is a graph showing the XRD measurement results of a common iron plate and a silicon-coated iron plate of the present invention before and after heat treatment.
[0046] Figure 3 The following are photographs showing the results of SEM measurement of a conventional iron plate and a silicon-coated iron plate of the present invention before and after heat treatment.
[0047] Figure 4 Part (a) is the TEM cross-sectional measurement result of the silicon-coated iron plate of the present invention, and parts (b) and (c) are photographs and graphs showing the TEM component analysis results of the sample surface.
[0048] Figure 5It is a graph showing the surface resistance measurement results of a conventional iron plate and a silicon-coated iron plate of the present invention before and after heat treatment.
[0049] Figure 6 The diagram is a predicted distribution diagram of oxygen (red) and silicon (blue) on the iron (gold) thin film of the silicon-coated iron plate of the present invention, wherein part (a) is a photograph showing a side view, and part (b) is a photograph showing a top view.
[0050] Figure 7 It is a graph showing the ΔE and atomic distribution prediction diagram of ordinary iron plate and silicon-coated iron plate of the present invention as the penetration depth changes.
[0051] Figure 8 These are photos of ordinary nickel plates and silicon (Si) coated nickel plates before and after heat treatment.
[0052] Fig. 9 The graph shows the XRD measurement results of the ordinary nickel plate and the silicon-coated nickel plate of the present invention before and after heat treatment.
[0053] Fig.10 The following are photographs showing the SEM measurement results of ordinary nickel plates and silicon-coated nickel plates before and after heat treatment.
[0054] Fig.11 Part (a) is the TEM cross-sectional measurement result of the silicon-coated nickel plate of the present invention, and parts (b) and (c) are photographs and graphs showing the TEM component analysis results of the sample surface.
[0055] Fig.12 The graph is a graph showing the surface resistance measurement results of a common nickel plate and a silicon-coated nickel plate of the present invention before and after heat treatment.
[0056] Fig.13 This is a predicted distribution diagram of oxygen (red) and silicon (gray) on the nickel (green) film of the silicon-nickel coated plate of the present invention, part (a) is a photograph showing a side view, and part (b) is a photograph showing a top view.
[0057] Fig.14 It is a graph showing the ΔE and atomic distribution prediction diagram of ordinary nickel plate and silicon-coated nickel plate of the present invention as the penetration depth changes. DETAILED DESCRIPTION
[0058] In this specification, the terms used are currently widely used common terms selected as much as possible in consideration of the functions of the present invention, but this may be different depending on the intention or practice of ordinary technicians in the technical field to which the present invention belongs, the emergence of new technologies, etc. In addition, in certain cases, the applicant may also arbitrarily select terms, in which case their meanings are described in detail in the description of the relevant invention. Therefore, in the present invention, the terms used should be defined based on the meaning of the terms and the overall content of the present invention, rather than just based on the names of the terms.
[0059] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs. Terms defined in commonly used dictionaries should be interpreted as meanings that are the same as those in the context of the relevant technology and should not be interpreted as idealized or overly formalized unless clearly defined in this application.
[0060] Numerical ranges include the values defined in the above ranges. In this specification, any maximum numerical limit provided includes all lower numerical limits that explicitly record lower numerical limits. In this specification, any minimum numerical limit provided includes all higher numerical limits that explicitly record higher numerical limits. In this specification, all numerical limits provided include all numerical ranges in which narrower numerical limit ranges and wider numerical ranges are explicitly recorded.
[0061] Silicon-coated anti-oxidation iron
[0062] The invention relates to silicon-coated anti-oxidation iron, in which a silicon (Si)-oxygen (O)-iron (Fe) mixed layer is formed on the silicon-coated anti-oxidation iron by evaporating silicon.
[0063] The anti-oxidation iron having the mixed layer can maintain electrical characteristics and have anti-oxidation characteristics.
[0064] Since the mixed layer is formed, additional oxidation other than the iron oxide layer can be prevented and oxidation resistance under high temperature conditions can be exhibited. The silicon is bonded to the oxygen on the iron surface and can be fixed on the iron surface. In this case, the most basic structure is as follows Figure 6 As shown. Figure 6 As shown in the side view shown in part (a) and the top view shown in part (b), after the oxygen covers the surface of the iron, if it is fixed via the silicon, other oxygen cannot enter the interior of the iron, thereby being able to exhibit oxidation resistance.
[0065] In the present invention, the resistance of the silicon-coated anti-oxidation iron may be between iron without the silicon (Si) being vapor-deposited and gold (Au).
[0066] In the present invention, the silicon-coated anti-oxidation iron may be a polycrystalline film, foil or block.
[0067] In the present invention, if the silicon-coated anti-oxidation iron is a polycrystalline film, foil or block, oxidation can be prevented even when heated at a temperature of 200° C. to 400° C. for 20 minutes to 40 minutes. In the case of the polycrystalline film, foil or block, oxidation is prevented, and even if the heat treatment is performed, the color confirmed by the naked eye, the XRD measurement, and the SEM measurement results do not change.
[0068] The present invention relates to a silicon-coated anti-oxidation iron, wherein a ferrosilicon alloy layer is formed on the anti-oxidation iron of the present invention, and the ferrosilicon alloy layer is a silicon (Si)-oxygen (O)-iron (Fe) mixed layer formed by silicon vapor deposition.
[0069] The oxidation-resistant iron formed with the above-mentioned ferrosilicon alloy layer can maintain the electrical and magnetic properties and has oxidation-resistant properties.
[0070] Since the silicon-iron alloy layer is formed, it is possible to prevent additional oxidation other than the iron oxide layer and exhibit oxidation resistance under high temperature conditions. The silicon is bonded to the oxygen on the iron surface and can be fixed on the iron surface. In this case, the most basic structure is as follows Figure 6 As shown. Figure 6 As shown in the side view shown in part (a) and the top view shown in part (b), after the oxygen covers the surface of the iron, if it is fixed via the silicon, other oxygen cannot enter the interior of the iron, thereby being able to exhibit oxidation resistance.
[0071] In the present invention, the resistance of the silicon-coated anti-oxidation iron may be similar to that of iron without the silicon (Si) being vapor-deposited.
[0072] In the present invention, the silicon-coated anti-oxidation iron can be a film, foil or block.
[0073] In the present invention, if the silicon-coated anti-oxidation iron is a polycrystalline thin film, foil or block, oxidation can be prevented even if heated at a temperature of 200° C. to 350° C. for 20 minutes to 40 minutes. In the case of the thin film, foil or block, oxidation is prevented, and even if the heat treatment is performed, the color confirmed by the naked eye, the XRD measurement, and the SEM measurement results do not change.
[0074] In the present invention, the surface resistance value of the silicon-coated anti-oxidation iron can be 9.2×10 -4 Ω / □ to 9.6×10 -4 The surface resistance value of the silicon-coated anti-oxidation iron can be similar to that of iron without silicon coating, and the surface resistance value does not increase sharply even after heat treatment.
[0075] In the present invention, the silicon-coated anti-oxidation iron may include: an iron layer 10; an iron oxide (Fe3O4) layer 20 formed on the upper end of the iron layer 10; a ferrosilicon alloy layer 30 formed by a mixture of silicon (Si)-oxygen (O)-iron (Fe) on the upper end of the iron oxide layer 20; and a silicon (Si)-oxygen (O) mixed layer 40 formed on the upper end of the ferrosilicon alloy layer 30.
[0076] In the present invention, the thickness of the iron oxide (Fe3O4) layer 20 may be 3 nm to 7 nm, preferably 3 nm to 5 nm. The iron oxide layer may be formed very thin so as to hardly affect the corrosion resistance of iron.
[0077] In the present invention, the thickness of the ferrosilicon alloy layer 30 formed by mixing the above silicon (Si)-oxygen (O)-iron (Fe) can be 0.8 nm to 1.2 nm.
[0078] In the present invention, the thickness of the silicon (Si)-oxygen (O) mixed layer 40 may be 5 nm to 30 nm, and preferably, may be 8 mm to 20 mm.
[0079] Preparation method of silicon-coated anti-oxidation iron
[0080] The invention relates to a method for preparing silicon-coated anti-oxidation iron.
[0081] The silicon-coated anti-oxidation iron of the present invention forms a ferrosilicon alloy layer, and the ferrosilicon alloy layer is a silicon (Si)-oxygen (O)-iron (Fe) mixed layer formed by silicon vapor deposition.
[0082] The oxidation-resistant iron formed with the above-mentioned silicon-iron alloy layer can maintain electrical characteristics and have oxidation-resistant properties.
[0083] Since the mixed layer is formed, additional oxidation other than the iron oxide layer can be prevented and oxidation resistance under high temperature conditions can be exhibited. The silicon is bonded to the oxygen on the iron surface and can be fixed on the iron surface. In this case, the most basic structure is as follows Figure 6 As shown. Figure 6 As shown in the side view shown in part (a) and the top view shown in part (b), after the oxygen covers the surface of the iron, if it is fixed via the silicon, other oxygen cannot enter the interior of the iron, thereby being able to exhibit oxidation resistance.
[0084] In the present invention, the resistance of the silicon-coated anti-oxidation iron may be similar to that of iron without the silicon (Si) being vapor-deposited.
[0085] In the present invention, the silicon-coated anti-oxidation iron can be a film, foil or block.
[0086] In the present invention, if the silicon-coated anti-oxidation iron is a film, foil or block, oxidation can be prevented even when heated at a temperature of 200° C. to 350° C. for 20 minutes to 40 minutes. In the case of the film, foil or block, oxidation is prevented, and even if the heat treatment is performed, the color confirmed by the naked eye, the XRD measurement, and the SEM measurement results do not change.
[0087] In the present invention, the surface resistance of the silicon-coated anti-oxidation iron can be 9.2×10 -4 Ω / □ to 9.6×10 -4 The surface resistance of the silicon-coated anti-oxidation iron can be similar to that of iron without silicon coating, and the surface resistance does not increase sharply even after heat treatment.
[0088] In the present invention, the silicon-coated anti-oxidation iron may include: an iron layer 10; an iron oxide (Fe3O4) layer 20 formed on the upper end of the iron layer 10; a ferrosilicon alloy layer 30 formed by a mixture of silicon (Si)-oxygen (O)-iron (Fe) on the upper end of the iron oxide layer 20; and a silicon (Si)-oxygen (O) mixed layer 40 formed on the upper end of the ferrosilicon alloy layer 30.
[0089] In the present invention, the thickness of the iron oxide (Fe3O4) layer 20 may be 3 nm to 7 nm. The iron oxide layer may be formed very thin so as not to affect the corrosion resistance of iron.
[0090] In the present invention, the thickness of the ferrosilicon alloy layer 30 formed by mixing the above silicon (Si)-oxygen (O)-iron (Fe) can be 0.8 nm to 1.2 nm.
[0091] In the present invention, the thickness of the silicon (Si)-oxygen (O) mixed layer 40 may be 5 nm to 30 nm, and preferably, may be 8 mm to 20 mm.
[0092] The present invention relates to a method for preparing silicon-coated anti-oxidation iron by depositing silicon (Si) onto iron (Fe) through a single-step sputtering process. As described above, since the single-step process is performed, the preparation method can be very simple and economical.
[0093] In the present invention, the sputtering may be performed under an argon atmosphere.
[0094] In the present invention, the sputtering may be performed for 1 minute to 5 minutes at a temperature of room temperature to 350° C., and preferably, for 70 seconds to 350 seconds at a temperature of 180° C. to 200° C. When the sputtering is performed, if the temperature and the execution time are higher or lower than the range, the crystallinity decreases as the grain boundary and the potential are formed, and therefore, it is preferably performed within the range of the temperature and the execution time.
[0095] Silicon-coated anti-oxidation nickel
[0096] The present invention relates to silicon-coated anti-oxidation nickel, which forms a silicon-nickel alloy layer 200. The silicon-nickel alloy layer is a silicon (Si)-oxygen (O)-iron (Fe) mixed layer formed by silicon vapor deposition.
[0097] The oxidation-resistant nickel formed with the silicon-nickel alloy layer 200 can maintain electrical properties and have oxidation-resistant properties.
[0098] Since the silicon-nickel alloy layer is formed, oxidation can be prevented and oxidation resistance under high temperature conditions can be exhibited. The silicon is bonded to the oxygen on the surface of the nickel layer and can be fixed on the nickel surface. In this case, the most basic structure is as follows Figure 6 As shown. Figure 6 As shown in the side view shown in part (a) and the top view shown in part (b), after the oxygen covers the surface of the nickel, if it is fixed via the silicon, other oxygen cannot enter the interior of the nickel, thereby being able to exhibit oxidation resistance.
[0099] In the present invention, if the silicon-coated oxidation-resistant nickel is a single-crystal thin film, it can be prevented from being oxidized even when heated at a temperature of 300° C. to 500° C. for 20 minutes to 50 minutes.
[0100] In the present invention, if the silicon-coated anti-oxidation nickel is a polycrystalline film, foil or block, oxidation can be prevented even when heated at a temperature of 200° C. to 400° C. for 20 minutes to 50 minutes. In the case of the polycrystalline film, foil or block, oxidation is prevented, and even if the heat treatment is performed, the color confirmed by the naked eye, the XRD measurement, and the SEM measurement results do not change.
[0101] In the present invention, the surface resistance value of the silicon-coated anti-oxidation nickel can be 6.2×10 -4 Ω / □ to 6.8×10 -4 The surface resistance value of the silicon-coated anti-oxidation nickel can be similar to that of nickel not coated with silicon, and the surface resistance value does not increase sharply even after heat treatment.
[0102] In the present invention, the above-mentioned silicon-coated anti-oxidation nickel may include: a nickel layer 100; a silicon-nickel alloy layer 200, formed by a mixture of silicon (Si)-oxygen (O)-nickel (Ni) on the upper end of the above-mentioned nickel layer 100; a first silicon (Si)-oxygen (O) mixed layer 300, formed on the upper end of the above-mentioned silicon-nickel alloy layer 200; and a second silicon (Si)-oxygen (O) mixed layer 400, formed on the upper end of the above-mentioned first silicon (Si)-oxygen (O) mixed layer 300.
[0103] In the present invention, the thickness of the silicon-nickel alloy layer 200 may be 0.8 nm to 1.2 nm.
[0104] In the present invention, the thickness of the silicon (Si)-oxygen (O) mixed layer including the first silicon (Si)-oxygen (O) mixed layer 300 and the second silicon (Si)-oxygen (O) mixed layer 400 may be 5 nm to 30 nm, preferably 8 nm to 20 nm. In the first silicon (Si)-oxygen (O) mixed layer 300, the oxygen content may be higher than the nickel content, and in the second silicon (Si)-oxygen (O) mixed layer 400, the nickel content may be higher than the oxygen content.
[0105] Preparation method of silicon-coated anti-oxidation nickel
[0106] The invention relates to a method for preparing silicon-coated anti-oxidation nickel.
[0107] The silicon-coated anti-oxidation nickel of the present invention is formed with a silicon-nickel alloy layer 200, wherein the silicon-nickel alloy layer 200 is a silicon (Si)-oxygen (O)-nickel (Ni) mixed layer formed by silicon evaporation. The present invention relates to a preparation method of silicon-coated anti-oxidation nickel.
[0108] The present invention relates to oxidation-resistant nickel. The silicon-coated oxidation-resistant nickel of the present invention forms a silicon-nickel alloy layer 200. The silicon-nickel alloy layer 200 is a silicon (Si)-oxygen (O)-nickel (Ni) mixed layer formed by silicon vapor deposition.
[0109] The oxidation-resistant nickel formed with the silicon-nickel alloy layer 200 can maintain electrical properties and have oxidation-resistant properties.
[0110] Since the silicon-nickel alloy layer is formed, oxidation can be prevented and oxidation resistance under high temperature conditions can be exhibited. The silicon is bonded to the oxygen on the surface of the nickel layer and can be fixed on the nickel surface. In this case, the most basic structure is as follows Figure 6 As shown. Figure 6 As shown in the side view shown in part (a) and the top view shown in part (b), after the oxygen covers the surface of the nickel, if it is fixed via the silicon, other oxygen cannot enter the interior of the nickel, thereby being able to exhibit oxidation resistance.
[0111] In the present invention, the resistance of the silicon-coated anti-oxidation nickel may be similar to that of nickel without the silicon (Si) being evaporated.
[0112] In the present invention, the silicon-coated anti-oxidation nickel may be a single crystal film, a polycrystalline film, a foil or a block.
[0113] In the present invention, if the silicon-coated oxidation-resistant nickel is a single-crystal thin film, it can be prevented from being oxidized even when heated at a temperature of 300° C. to 500° C. for 20 minutes to 50 minutes.
[0114] In the present invention, if the silicon-coated anti-oxidation nickel is a polycrystalline film, foil or block, oxidation can be prevented even when heated at a temperature of 200° C. to 400° C. In the case of the polycrystalline film, foil or block, oxidation is prevented, and even if the heat treatment is performed, the color confirmed by the naked eye, the XRD measurement, and the SEM measurement results do not change.
[0115] In the present invention, the surface resistance value of the silicon-coated anti-oxidation nickel can be 6.2×10 -4 Ω / □ to 6.8×10 -4 The surface resistance value of the silicon-coated anti-oxidation nickel can be similar to that of nickel not coated with silicon, and the surface resistance value does not increase sharply even after heat treatment.
[0116] In the present invention, the above-mentioned silicon-coated anti-oxidation nickel may include: a nickel layer 100; a silicon-nickel alloy layer 200, formed by a mixture of silicon (Si)-oxygen (O)-nickel (Ni) on the upper end of the above-mentioned nickel layer 100; a first silicon (Si)-oxygen (O) mixed layer 300, formed on the upper end of the above-mentioned silicon-nickel alloy layer 200; and a second silicon (Si)-oxygen (O) mixed layer 400, formed on the upper end of the above-mentioned first silicon (Si)-oxygen (O) mixed layer 300.
[0117] In the present invention, the thickness of the silicon-nickel alloy layer 200 may be 0.8 nm to 1.2 nm.
[0118] The thickness of the silicon (Si)-oxygen (O) mixed layer including the first silicon (Si)-oxygen (O) mixed layer 300 and the second silicon (Si)-oxygen (O) mixed layer 400 may be 5 nm to 30 nm, preferably 8 nm to 20 nm. In the first silicon (Si)-oxygen (O) mixed layer 300, the oxygen content may be higher than the nickel content, and in the second silicon (Si)-oxygen (O) mixed layer 400, the nickel content may be higher than the oxygen content.
[0119] The present invention relates to a method for preparing silicon-coated anti-oxidation nickel by depositing silicon (Si) onto nickel (Ni) in a single-step sputtering process. As described above, since the single-step process is performed, the preparation method can be very simple and economical.
[0120] In the present invention, the sputtering may be performed under an argon atmosphere.
[0121] In the present invention, the sputtering may be performed for 1 minute to 5 minutes at a temperature of room temperature to 350° C., and preferably, for 70 seconds to 350 seconds at a temperature of 180° C. to 200° C. When the sputtering is performed, if the temperature and the execution time are higher or lower than the range, the crystallinity decreases as the grain boundary and the potential are formed, and therefore, it is preferably performed within the range of the temperature and the execution time.
[0122] Example
[0123] Hereinafter, examples of the present invention will be described in detail, but it is obvious that the present invention is not limited to the following examples.
[0124] The advantages, features and implementation methods of the present invention can be clearly understood by referring to the embodiments described in detail. However, the present invention is not limited to the embodiments disclosed below and can be implemented by different implementation methods. The embodiments of the present invention are only used to make the disclosure of the present invention complete so that ordinary technicians in the technical field to which the present invention belongs can fully understand the scope of the present invention. The present invention should be defined based on the scope of protection claimed by the invention.
[0125] Example 1. Silicon-coated iron plate
[0126] In an argon atmosphere, 20 nm of silicon (Si) was deposited on an iron (Fe) plate by sputtering at 190° C. for 5 minutes to prepare a silicon-coated anti-oxidation iron plate.
[0127] Comparative Example 1. Iron plate without silicon coating
[0128] An iron plate not coated with silicon was prepared.
[0129] Example 2. Silicon-coated nickel plate
[0130] In an argon atmosphere, 20 nm of silicon (Si) was deposited on a nickel (Ni) plate by sputtering at 190° C. for 5 minutes to prepare a silicon-coated anti-oxidation iron plate.
[0131] Comparative Example 2. Nickel plate without silicon coating
[0132] A nickel plate not coated with silicon was prepared.
[0133] Experimental Example 1. Observation of oxidation degree after heat treatment
[0134] The iron plates prepared in Example 1 and Comparative Example 1 were heat treated at 300°C for 30 minutes and the states before and after the heat treatment were observed. Figure 1 shown.
[0135] like Figure 1As shown, the iron plate of Comparative Example 1 darkened due to oxidation after heat treatment, whereas the silicon-coated anti-oxidation iron plate prepared in Example 1 maintained its initial color even after heat treatment, thereby confirming that no oxidation occurred.
[0136] Based on the results described above, it was confirmed that the silicon-coated antioxidant iron of the present invention has antioxidant properties.
[0137] Furthermore, the nickel plates prepared in Example 2 and Comparative Example 1 were heat treated at 400°C for 30 minutes and the states before and after the heat treatment were observed. Figure 8 shown.
[0138] like Figure 8 As shown, the nickel plate of Comparative Example 2 darkened due to oxidation after heat treatment, whereas the silicon-coated anti-oxidation nickel plate prepared in Example 2 maintained its initial color even after heat treatment, thereby confirming that no oxidation occurred.
[0139] Based on the above results, it was confirmed that the silicon-coated antioxidant nickel of the present invention has antioxidant properties.
[0140] Experimental Example 2. XRD measurement
[0141] The iron plates prepared in Example 1 and Comparative Example 1 were heat treated at 300°C for 30 minutes and the states before and after the heat treatment were measured by XRD. The results are as follows: Figure 2 shown.
[0142] like Figure 2 As shown, the silicon-coated anti-oxidation iron plate prepared in Example 1 showed no peaks other than iron (Fe) before and after heat treatment. In addition, the crystal structure remained unchanged. It was confirmed that the silicon-coated anti-oxidation iron plate was hardly oxidized after heat treatment. On the contrary, the iron plate of Comparative Example 1 was confirmed to be oxidized after heat treatment due to the generation of an iron oxide peak. In the above Example 1, although iron oxide (Fe3O4) was presumed to be generated, it was judged that it did not appear in the XRD results because there was almost no oxidation reaction and it was generated very thinly.
[0143] Based on the results described above, it was confirmed that the silicon-coated antioxidant iron of the present invention has antioxidant properties.
[0144] Furthermore, the nickel plates prepared in Example 2 and Comparative Example 2 were heat treated at 400°C for 30 minutes and the states before and after the heat treatment were measured by XRD. The results are as follows: Fig. 9 shown.
[0145] like Fig. 9As shown, the silicon-coated anti-oxidation nickel plate prepared in Example 2 showed no peaks other than nickel (Ni) before and after heat treatment. In addition, the crystal structure remained unchanged. It was thus confirmed that the silicon-coated anti-oxidation nickel plate was hardly oxidized after heat treatment. On the contrary, the nickel plate of Comparative Example 2 was oxidized after heat treatment due to the generation of nickel oxide peaks.
[0146] Based on the above results, it was confirmed that the silicon-coated antioxidant nickel of the present invention has antioxidant properties.
[0147] Experimental Example 3. SEM Observation
[0148] The iron plates prepared in Example 1 and Comparative Example 1 were heat treated at 300°C for 30 minutes and observed by SEM magnified 10,000 times before and after the heat treatment. Figure 3 shown.
[0149] like Figure 3 As shown, after the heat treatment, the iron plate of Comparative Example 1 has a change on the surface, while the silicon-coated anti-oxidation iron plate prepared in Example 1 has no change even after the heat treatment. Therefore, it is confirmed that the silicon-coated anti-oxidation iron plate of Example 1 is not oxidized.
[0150] Based on the results described above, it was confirmed that the silicon-coated antioxidant iron of the present invention has antioxidant properties.
[0151] Furthermore, the nickel plates prepared in Example 2 and Comparative Example 2 were heat treated for 30 minutes at 400°C and observed by SEM magnified 10,000 times before and after the heat treatment. Fig.10 shown.
[0152] like Fig.10 As shown, after heat treatment, the nickel plate of Comparative Example 2 undergoes changes on the surface, whereas the silicon-coated anti-oxidation nickel plate prepared in Example 2 does not undergo any changes even after heat treatment. Thus, it is confirmed that the silicon-coated anti-oxidation nickel plate prepared in Example 2 does not undergo oxidation.
[0153] Based on the above results, it was confirmed that the silicon-coated antioxidant nickel of the present invention has antioxidant properties.
[0154] Experimental Example 4. TEM Analysis
[0155] The iron plate prepared in Example 1 was analyzed by TEM, and the results were as follows: Figure 4 shown.
[0156] like Figure 4As shown, the silicon-coated anti-oxidation iron plate forms a thin film surface in the order of an iron layer, an iron oxide (Fe3O4) layer formed on the upper end of the iron layer, a ferrosilicon alloy layer formed on the upper end of the iron oxide layer by a mixture of silicon (Si)-oxygen (O)-iron (Fe), and a silicon (Si)-oxygen (O) mixed layer formed on the upper end of the ferrosilicon alloy layer.
[0157] The iron plate forms a natural oxide film due to exposure to air and produces an iron oxide (Fe3O4) phase. However, the thickness of the natural oxide film is very thin and difficult to observe with the naked eye or show as XRD results. As silicon is evaporated on the natural oxide film, silicon atoms fix the oxygen that moves freely on the silicon surface at the best position (site) to represent the silicon-iron alloy layer. It is judged that the silicon-iron alloy layer plays a key role in preventing oxidation. The formation of silicon (Si)-oxygen (O)-iron (Fe) bonds was confirmed.
[0158] Based on the results described above, it was confirmed that the silicon-coated anti-oxidation iron of the present invention prevents oxidation by forming a silicon (Si)-oxygen (O)-iron (Fe) mixed layer on the iron layer and exhibits oxidation resistance under high temperature conditions.
[0159] Furthermore, the silicon-coated anti-oxidation nickel plate prepared in Example 2 was analyzed by TEM, and the results are as follows: Fig.11 shown.
[0160] like Fig.11 As shown, the silicon-coated anti-oxidation nickel plate forms a thin film surface in the order of a nickel layer, a silicon-nickel alloy layer formed on the upper end of the nickel layer by a mixture of silicon (Si)-oxygen (O)-nickel (Ni), a first silicon (Si)-oxygen (O) mixed layer formed on the upper end of the silicon-nickel alloy layer, and a second silicon (Si)-oxygen (O) mixed layer formed on the first silicon (Si)-oxygen (O) mixed layer.
[0161] As silicon is evaporated on the nickel layer, silicon atoms fix the oxygen that moves freely on the surface of the nickel layer at the optimal site to generate silicon (Si)-oxygen (O)-nickel (Ni) bonds. It is thus determined that the silicon-nickel alloy layer formed plays a key role in preventing oxidation.
[0162] Based on the results described above, it was confirmed that the silicon-coated oxidation-resistant nickel of the present invention prevents oxidation by forming a silicon (Si)-oxygen (O)-nickel (Ni) mixed layer on the nickel layer and exhibits oxidation resistance under high temperature conditions.
[0163] Experimental Example 5. Surface resistance measurement
[0164] The iron plates prepared in Example 1 and Comparative Example 1 were heat treated at 300°C for 30 minutes and the surface resistances before and after the heat treatment were measured. Figure 5 shown.
[0165] like Figure 5 As shown, the surface resistance value of the iron plate of Comparative Example 1 increases sharply after heat treatment, whereas the silicon-coated anti-oxidation iron plate prepared in Example 1 shows no significant change even after heat treatment.
[0166] Based on the above results, it was confirmed that the silicon-coated antioxidant iron of the present invention exhibited antioxidant properties while maintaining electrical properties.
[0167] Furthermore, the nickel plates prepared in Example 2 and Comparative Example 2 were heat treated at 400°C for 30 minutes and the surface resistances before and after the heat treatment were measured. Fig.12 shown.
[0168] like Fig.12 As shown, the surface resistance value of the iron plate of Comparative Example 2 increases sharply after heat treatment, while, in contrast, the silicon-coated anti-oxidation nickel plate prepared in Example 2 shows no significant change even after heat treatment.
[0169] Based on the above results, it was confirmed that the silicon-coated oxidation-resistant nickel of the present invention exhibits oxidation-resistant properties while maintaining electrical properties.
[0170] Experimental Example 6. Determination of oxygen energy difference based on penetration depth
[0171] Taking the energy of the surface state of the silicon-coated anti-oxidation iron plate prepared in Example 1 as the reference, when oxygen penetrates into the iron, the energy is calculated based on the depth from the surface. When oxygen exists on the surface of the sample, the difference from the calculated energy is as follows: Figure 7 shown.
[0172] like Figure 7 As shown, in the silicon-coated anti-oxidation iron plate prepared in the above Example 1, oxygen needs to cross an energy barrier in order to pass through the silicon (Si)-oxygen (O)-iron (Fe) mixed layer on the surface. The above energy barrier refers to oxidation resistance.
[0173] Based on the results described above, it was confirmed that the silicon-coated antioxidant iron of the present invention has antioxidant properties.
[0174] Furthermore, taking the energy of the surface state of the silicon-coated anti-oxidation nickel plate prepared in Example 2 as the reference, when oxygen penetrates into the nickel, the energy is calculated based on the depth from the surface. When oxygen exists on the surface of the sample, the difference from the calculated energy is as follows: Fig.14 shown.
[0175] like Fig.14 As shown, in the silicon-coated anti-oxidation nickel plate prepared in the above Example 2, oxygen needs to cross an energy barrier in order to pass through the silicon (Si)-oxygen (O)-nickel (Ni) mixed layer on the surface. The above energy barrier refers to oxidation resistance.
[0176] Based on the above results, it was confirmed that the silicon-coated antioxidant nickel of the present invention has antioxidant properties.
[0177] Description of Reference Numerals
[0178] 10: Iron layer
[0179] 20: Iron oxide (Fe3O4) layer
[0180] 30: Ferrosilicon alloy layer
[0181] 40: Silicon (Si)-oxygen (O) mixed layer
[0182] 100: Nickel (Ni) layer
[0183] 200: Silicon nickel alloy layer
[0184] 300: First silicon (Si)-oxygen (O) mixed layer
[0185] 400: Second silicon (Si)-oxygen (O) mixed layer
Claims
1. A silicon-coated antioxidant iron, characterized in that: A ferrosilicon alloy layer (30) is formed, wherein the ferrosilicon alloy layer is a silicon-oxygen-iron mixed layer formed by silicon vapor deposition.
2. The silicon-coated antioxidant iron according to claim 1, characterized in that: The electrical resistance of the silicon-coated anti-oxidation iron is similar to that of iron without the silicon vapor deposition.
3. The silicon-coated antioxidant iron according to claim 1, characterized in that: The silicon-coated anti-oxidation iron is in the form of a film, foil or block.
4. The silicon-coated antioxidant iron according to claim 3, characterized in that: When the silicon-coated anti-oxidation iron is in the form of a film, foil or block, it can be prevented from being oxidized even when heated at a temperature of 200° C. to 350° C. for 20 minutes to 40 minutes.
5. The silicon-coated antioxidant iron according to claim 1, characterized in that: The surface resistance of the silicon-coated anti-oxidation iron is 9.2×10 -4 Ω / □ to 9.6×10 -4 Ω / □.
6. The silicon-coated antioxidant iron according to claim 1, characterized in that: The above-mentioned ferrosilicon coating comprises: Iron layer (10); An iron oxide layer (20) formed on the upper end of the iron layer (10); a ferrosilicon alloy layer (30) formed by mixing silicon, oxygen and iron on the upper end of the iron oxide layer (20); and A silicon-oxygen mixed layer (40) is formed on the upper end of the above-mentioned silicon-iron alloy layer (30).
7. The silicon-coated antioxidant iron according to claim 6, characterized in that: The thickness of the iron oxide layer (20) is 3nm to 7nm.
8. The silicon-coated antioxidant iron according to claim 6, characterized in that: The thickness of the ferrosilicon alloy layer (30) formed by the above silicon-oxygen-iron mixture is 0.8nm to 1.2nm.
9. The silicon-coated antioxidant iron according to claim 6, characterized in that: The thickness of the silicon-oxygen mixed layer (40) is 5 nm to 30 nm.
10. A method for preparing silicon-coated antioxidant iron, characterized in that: Silicon is evaporated onto iron in a single-step sputtering process.
11. The method for preparing silicon-coated antioxidant iron according to claim 10, characterized in that: The above sputtering was performed under an argon atmosphere.
12. The method for preparing silicon-coated antioxidant iron according to claim 10, characterized in that: The sputtering is performed at a temperature ranging from room temperature to 350° C. for 1 minute to 5 minutes.
13. A silicon-coated anti-oxidation nickel, characterized in that: A silicon-nickel alloy layer (200) is formed, wherein the silicon-nickel alloy layer is a silicon-oxygen-nickel mixed layer formed by silicon vapor deposition.
14. The silicon-coated anti-oxidation nickel according to claim 13, characterized in that: The electrical resistance of the silicon-coated anti-oxidation nickel is similar to that of the nickel not deposited as specified above.
15. The silicon-coated anti-oxidation nickel according to claim 13, characterized in that: The silicon-coated anti-oxidation nickel is in the form of a single crystal film, a polycrystalline film, a foil or a block.
16. The silicon-coated anti-oxidation nickel according to claim 15, characterized in that: When the silicon-coated anti-oxidation nickel is a single crystal thin film, it can be prevented from being oxidized even when heated at a temperature of 300° C. to 500° C. for 20 minutes to 50 minutes.
17. The silicon-coated anti-oxidation nickel according to claim 15, characterized in that: When the silicon-coated oxidation-resistant nickel is in the form of a polycrystalline thin film, foil or block, it can be prevented from being oxidized even when heated at a temperature of 200°C to 400°C.
18. The silicon-coated anti-oxidation nickel according to claim 13, characterized in that: The surface resistance of the silicon-coated anti-oxidation nickel is 6.2×10 -4 Ω / □ to 6.8×10 -4 Ω / □.
19. The silicon-coated anti-oxidation nickel according to claim 13, characterized in that: The above-mentioned silicon-nickel coating includes: Nickel layer (100); A silicon-nickel alloy layer (200) formed by mixing silicon-oxygen-nickel on the upper end of the nickel layer (100); A first silicon-oxygen mixed layer (300) is formed on the upper end of the silicon-nickel alloy layer (200); and The second silicon-oxygen mixed layer (400) is formed on the upper end of the first silicon-oxygen mixed layer (300).
20. The silicon-coated anti-oxidation nickel according to claim 19, characterized in that: The thickness of the silicon-nickel alloy layer (200) is 0.8 nm to 1.2 nm.
21. The silicon-coated anti-oxidation nickel according to claim 19, characterized in that: The thickness of the silicon-oxygen mixed layer including the first silicon-oxygen mixed layer (300) and the second silicon-oxygen mixed layer (400) is 5 nm to 30 nm.
22. A method for preparing silicon-coated anti-oxidation nickel, characterized in that: Silicon is evaporated onto nickel in a single-step sputtering process.
23. The method for preparing silicon-coated anti-oxidation nickel according to claim 22, characterized in that: The above sputtering was performed under an argon atmosphere.
24. The method for preparing silicon-coated anti-oxidation nickel according to claim 22, characterized in that: The sputtering is performed at a temperature ranging from room temperature to 350° C. for 1 minute to 5 minutes.