Photosensitive resin composition, photosensitive element, printed wiring board, and method for producing printed wiring board
By using acid-modified photosensitive resin compositions containing materials such as vinyl resins and organosilane compounds, combined with light development technology, the problem of insufficient performance of permanent resist in printed circuit boards is solved, and high resolution and heat resistance are achieved , suitable for the manufacturing of high-density printed circuit boards.
Patent Information
- Application Number
- CN202380035618.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-12-21
- Filing Date
- 2023-12-20
- Publication Date
- 2024-12-03
AI Technical Summary
The permanent resist of the existing printed circuit boards has shortcomings in high density and fine pattern formation, heat shock resistance, heat resistance and insulation, making it difficult to take into account high performance.
The performance of the inorganic filler is improved by surface treatment of the filler and through specific light development techniques using a photosensitive resin composition containing acid-modified vinyl-containing resin, photopolymerizable compound, photopolymerization initiator, inorganic filler and organic silane compound. Form a high-performance permanent resist.
It realizes a permanent resist with excellent high resolution, heat shock resistance, heat resistance and insulation. It is suitable for the manufacturing of high-density printed circuit boards, and improves circuit adhesion and insulation reliability.
Smart Images

Figure BDA0005095836800000061 
Figure BDA0005095836800000062 
Figure BDA0005095836800000071
Abstract
Description
Technical Field
[0001] The present invention relates to a photosensitive resin composition for permanent resist, a photosensitive element, a printed circuit board and a method for manufacturing the printed circuit board. Background Art
[0002] In the field of printed wiring boards, a process for forming a permanent resist on a printed wiring board is currently underway. The permanent resist prevents corrosion of the conductor layer during use of the printed wiring board and maintains electrical insulation between conductor layers. In recent years, the permanent resist has also served as a solder resist film, preventing solder from adhering to unnecessary portions of the conductor layer of the printed wiring board during processes such as flip-chip mounting and wire bonding of semiconductor elements onto the printed wiring board using solder.
[0003] Conventionally, permanent resists have been produced using screen printing with thermosetting resin compositions or photographic methods using photosensitive resin compositions. For example, in flexible circuit boards using mounting methods such as FC (Flip Chip), TAB (Tape Automated Bonding), and COF (Chip on Film), a permanent resist is formed by screen printing a thermosetting resin paste and then thermally curing it, excluding the IC chip, electronic components, LCD (Liquid Crystal Display) panel, and interconnecting wiring patterns (see, for example, Patent Document 1).
[0004] In semiconductor package substrates such as BGA (ball grid array) and CSP (chip size package) that are mounted on electronic components, it is necessary to remove the permanent resist at the bonding portion (1) in order to flip-chip mount the semiconductor element on the semiconductor package substrate via solder, (2) in order to wire-bond the semiconductor element to the semiconductor package substrate, and (3) in order to solder the semiconductor package substrate to the motherboard substrate. In the formation of an image of the permanent resist, a photographic method is used in which a photosensitive resin composition is applied and dried, then selectively irradiated with active light such as ultraviolet rays to cure it, and then developed to remove only the unirradiated portion to form an image. The photographic method is suitable for mass production due to its good operability and is therefore widely used in the electronic materials industry for forming images of photosensitive materials (e.g., see Patent Document 2).
[0005] Previous technical literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 2003-198105
[0008] Patent Document 2: Japanese Patent Application Laid-Open No. 11-240930 Summary of the Invention
[0009] Technical issues to be solved by the invention
[0010] In response to the increasing density of printed wiring boards, permanent resists are also being required to have further improved performance. In particular, a high degree of balance between fine pattern formability (resolution), thermal shock resistance, heat resistance, and insulation properties is being required.
[0011] An object of the present invention is to provide a photosensitive resin composition capable of forming a permanent resist having excellent resolution, thermal shock resistance, heat resistance, and insulation properties, a photosensitive element using the photosensitive resin composition, a printed wiring board, and a method for producing a printed wiring board.
[0012] Means for solving technical problems
[0013] One embodiment of the present invention relates to the following photosensitive resin composition, photosensitive element, printed wiring board, and method for producing the printed wiring board.
[0014] [1] A photosensitive resin composition for a permanent resist, comprising: (A) an acid-modified vinyl-containing resin, (B) a photopolymerizable compound, (C) a photopolymerization initiator, (D) an inorganic filler, and (E) an organosilane compound, wherein the inorganic filler (D) includes a surface-treated filler.
[0015] [2] The photosensitive resin composition according to [1] above, wherein
[0016] The surface-treated filler is an inorganic filler that has been surface-treated with at least one surface-treating agent selected from the group consisting of organic zirconium compounds, organic titanium compounds, organic aluminum compounds, and organic silane compounds.
[0017] [3] The photosensitive resin composition according to [1] or [2] above, wherein
[0018] The (E) organosilane compound contains at least one selected from the group consisting of epoxy silane compounds, amino silane compounds, mercapto silane compounds, (meth)acrylic silane compounds, vinyl silane compounds, alkyl silane compounds, isocyanate group-containing silane compounds, isocyanurate group-containing silane compounds, fluorene skeleton-containing silane compounds, and benzotriazole group-containing silane compounds.
[0019] [4] The photosensitive resin composition according to any one of [1] to [3] above, wherein
[0020] The content of the (E) organosilane compound is 1 to 40 parts by mass relative to 100 parts by mass of the (A) acid-modified vinyl-containing resin.
[0021] [5] The photosensitive resin composition according to any one of [1] to [4] above, wherein
[0022] (C) The photopolymerization initiator contains at least one selected from the group consisting of acetophenone compounds, thioxanthone compounds, benzophenone compounds, oxime ester compounds, and acylphosphine oxide compounds.
[0023] [6] A photosensitive element comprising a support film and a photosensitive layer formed on the support film, wherein the photosensitive layer contains the photosensitive resin composition according to any one of [1] to [5].
[0024] [7] A printed wiring board comprising a permanent resist containing a cured product of the photosensitive resin composition according to any one of [1] to [5].
[0025] [8] A method for manufacturing a printed wiring board, comprising: forming a photosensitive layer on a substrate using the photosensitive resin composition described in any one of [1] to [5] above; exposing and developing the photosensitive layer to form a resist pattern; and curing the resist pattern to form a permanent resist.
[0026] [9] A method for manufacturing a printed wiring board, comprising: forming a photosensitive layer on a substrate using the photosensitive element described in [6] above; exposing and developing the photosensitive layer to form a resist pattern; and curing the resist pattern to form a permanent resist.
[0027] Effects of the Invention
[0028] The present invention provides a photosensitive resin composition capable of forming a permanent resist having excellent resolution, thermal shock resistance, heat resistance, and insulation properties, a photosensitive element using the photosensitive resin composition, a printed wiring board, and a method for producing a printed wiring board. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a cross-sectional view schematically showing the photosensitive element of this embodiment. DETAILED DESCRIPTION
[0030] Hereinafter, an embodiment of the present invention will be described in detail, but the present invention is not limited thereto. In the following embodiments, unless otherwise expressly stated or clearly considered to be necessary in principle, the constituent elements (including element steps, etc.) are not essential. The same applies to numerical values and ranges thereof, and the present invention is not improperly limited thereto.
[0031] In the present invention, the term "layer" includes not only structures of shapes formed on the entire surface, but also structures of shapes formed on a part thereof when viewed from above. In the present invention, the term "process" includes not only independent processes, but also processes that achieve the intended purpose of the process even if they cannot be clearly distinguished from other processes. In the present invention, the numerical range represented by "to" represents a range that includes the numerical values recorded before and after "to" as the minimum and maximum values, respectively. In the numerical ranges described in stages in the present invention, the upper limit or lower limit of the numerical range of a certain stage can be replaced by the upper limit or lower limit of the numerical range of other stages. In addition, in the numerical ranges described in the present invention, the upper limit or lower limit of its numerical range can be replaced by the value shown in the embodiment. In the present invention, "A or B" includes either A or B, or both. With regard to the materials exemplified below, unless otherwise specified, one type can be used alone, or two or more types can be used in combination. In the present invention, when a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition refers to the total amount of the plurality of substances present in the composition unless otherwise specified.
[0032] In the present invention, "solid content" refers to non-volatile components after removing volatile substances such as water and diluent contained in the photosensitive resin composition, and means components that evaporate or remain when the resin composition is dried, and also includes components that are liquid, syrupy or waxy at room temperature (25°C, the same below).
[0033] [Photosensitive resin composition]
[0034] The photosensitive resin composition of this embodiment contains (A) an acid-modified vinyl-containing resin, (B) a photopolymerizable compound, (C) a photopolymerization initiator, (D) an inorganic filler, and (E) an organosilane compound, wherein the inorganic filler includes a surface-treated filler. The photosensitive resin composition of this embodiment is a negative-working photosensitive resin composition, and a cured film thereof can be suitably used as a permanent resist.
[0035] The photosensitive resin composition for permanent resists according to this embodiment can form permanent resists with excellent resolution, thermal shock resistance, heat resistance, and insulation properties. Furthermore, the photosensitive resin composition according to this embodiment exhibits excellent adhesion to inner layer circuits and electrical insulation reliability, as required for photosensitive resin compositions used in the manufacture of printed wiring boards, and is useful as interlayer insulating layers in multilayer printed wiring boards. The components contained in the photosensitive resin composition according to this embodiment are described in detail below.
[0036] <Component (A): Acid-modified vinyl-containing resin>
[0037] The photosensitive resin composition of the present embodiment contains an acid-modified vinyl-containing resin as component (A). The acid-modified vinyl-containing resin is not particularly limited as long as it has a vinyl bond which is a photopolymerizable ethylenically unsaturated bond and an alkali-soluble acidic group.
[0038] Examples of the group having an ethylenically unsaturated bond possessed by component (A) include a vinyl group, an allyl group, a propargyl group, a butenyl group, an ethynyl group, a phenylethynyl group, a maleimide group, a nadicimide group, and a (meth)acryloyl group. From the perspective of reactivity and resolution, the group having an ethylenically unsaturated bond may be a (meth)acryloyl group. Examples of the acidic group possessed by component (A) include a carboxyl group, a sulfo group, and a phenolic hydroxyl group. From the perspective of resolution, the acidic group may be a carboxyl group.
[0039] The component (A) may be an acid-modified vinyl-containing epoxy derivative obtained by reacting (a) an epoxy resin (hereinafter referred to as "component (a)") with (b) an organic acid containing an ethylenically unsaturated group (hereinafter referred to as "component (b)"), and (c) a polyacid anhydride containing a saturated or unsaturated group (hereinafter referred to as "component (c)").
[0040] Examples of acid-modified vinyl-containing epoxy derivatives include acid-modified epoxy (meth)acrylates. Acid-modified epoxy (meth)acrylates are resins obtained by acid-modifying epoxy (meth)acrylate, which is a reaction product of components (a) and (b), with component (c). Examples of acid-modified epoxy (meth)acrylates include those obtained by adding a saturated or unsaturated polybasic acid anhydride to an esterified product obtained by reacting an epoxy resin with a vinyl-containing monocarboxylic acid.
[0041] Examples of the component (A) include an acid-modified vinyl-containing resin (A1) (hereinafter referred to as "component (A1)") obtained by using a bisphenol novolac epoxy resin (a1) (hereinafter referred to as "epoxy resin (a1)") as the component (a), and an acid-modified vinyl-containing resin (A2) (hereinafter referred to as "component (A2)") obtained by using an epoxy resin (a2) other than the epoxy resin (a1) (hereinafter referred to as "epoxy resin (a2)") as the component (a). These can be used alone or in combination of two or more.
[0042] (Epoxy resin (a1))
[0043] Examples of the epoxy resin (a1) include epoxy resins having a structural unit represented by the following formula (I) or (II). The epoxy resin (a1) may be an epoxy resin having a structural unit represented by the formula (I).
[0044]
[0045] In formula (I), R 11 Represents a hydrogen atom or a methyl group, multiple R 11 Can be the same or different. 1 and Y 2 Each independently represents a hydrogen atom or a glycidyl group, but Y 1 and Y 2 At least one of them is a glycidyl group. From the viewpoint of suppressing the generation of undercuts and improving the linearity and resolution of the resist pattern profile, R 11 It can be a hydrogen atom. From the viewpoint of further improving the thermal shock resistance, Y 1 and Y 2 It may be a glycidyl group.
[0046] The number of structural units represented by formula (I) in the epoxy resin (a1) is 1 or more, and can be 10 to 100, 15 to 80, or 15 to 70. If the number of structural units is within the above range, it is easy to improve the linearity of the resist pattern profile, the adhesion to the copper substrate, the heat resistance, and the electrical insulation. Here, the number of structural units represents an integer value in a single molecule and represents a rational number as an average value in an aggregate of multiple molecules. Hereinafter, the number of structural units of the structural unit is also the same.
[0047]
[0048] In formula (II), R 12 Represents a hydrogen atom or a methyl group, multiple R 12 Can be the same or different. 3 and Y 4 Each independently represents a hydrogen atom or a glycidyl group, but Y 3 and Y 4 At least one of them is a glycidyl group. From the viewpoint of suppressing the generation of undercuts and improving the linearity and resolution of the resist pattern profile, R 12 It can be a hydrogen atom. From the viewpoint of further improving the thermal shock resistance, Y 3 and Y 4 It may be a glycidyl group.
[0049] The number of structural units represented by formula (II) in the epoxy resin (a1) is 1 or more, and can be 10 to 100, 15 to 80, or 15 to 70. When the number of structural units is within the above range, the linearity of the resist pattern profile, the adhesion to the copper substrate, and the heat resistance are easily improved.
[0050] In formula (II), R 12 is a hydrogen atom and Y 3 and Y 4 Epoxy resins having a glycidyl group are commercially available as EXA-7376 series (manufactured by DIC Corporation, trade name). 12 is methyl and Y 3 and Y 4 The epoxy resin which is a glycidyl group is commercially available as EPON SU8 series (manufactured by Mitsubishi Chemical Corporation, trade name).
[0051] (Epoxy resin (a2))
[0052] The epoxy resin (a2) is not particularly limited as long as it is an epoxy resin different from the epoxy resin (a1). From the viewpoint of suppressing the occurrence of undercuts and improving the linearity of the resist pattern profile, the adhesion to the copper substrate, and the resolution, the epoxy resin (a2) may be at least one selected from the group consisting of a novolac-type epoxy resin, a bisphenol A-type epoxy resin, a bisphenol F-type epoxy resin, a trisphenol methane-type epoxy resin, and a biphenyl-type epoxy resin.
[0053] Examples of novolac epoxy resins include epoxy resins having a structural unit represented by the following formula (III). Examples of bisphenol A epoxy resins or bisphenol F epoxy resins include epoxy resins having a structural unit represented by the following formula (IV). Examples of trisphenol methane epoxy resins include epoxy resins having a structural unit represented by the following formula (V). Examples of biphenyl epoxy resins include epoxy resins having a structural unit represented by the following formula (VI).
[0054] The epoxy resin (a2) is preferably a novolac-type epoxy resin having a structural unit represented by the following formula (III). Examples of the novolac-type epoxy resin having such a structural unit include a novolac-type epoxy resin represented by the following formula (III').
[0055]
[0056] In formula (III) and (III'), R 13 represents a hydrogen atom or a methyl group, Y 5represents a hydrogen atom or a glycidyl group, but Y 5 In formula (III'), n1 is a number greater than 1, and multiple R 13 and Y 5 From the viewpoint of suppressing the generation of undercuts and improving the linearity and resolution of the resist pattern profile, R 13 It may be a hydrogen atom.
[0057] From the viewpoint of suppressing the generation of undercuts and improving the linearity and resolution of the resist pattern profile, in formula (III'), Y as a hydrogen atom 5 With Y as glycidyl group 5 The molar ratio of n1 can be 0 / 100 to 30 / 70 or 0 / 100 to 10 / 90. n1 is 1 or more, but can also be 10 to 200, 30 to 150, or 30 to 100. When n1 is within the above range, the linearity of the resist pattern profile, the adhesion to the copper substrate, and the heat resistance are easily improved.
[0058] Examples of the novolac epoxy resin represented by formula (III') include phenol novolac epoxy resins and cresol novolac epoxy resins. These novolac epoxy resins can be obtained by reacting phenol novolac resins or cresol novolac resins with epichlorohydrin using a known method.
[0059] As the phenol novolac type epoxy resin or cresol novolac type epoxy resin represented by formula (III'), for example, YDCN-701, YDCN-702, YDCN-703, YDCN-704, YDCN-704L, YDPN-638, YDPN-602 (above are manufactured by NIPPON STEEL Chemical & Material Co., Ltd., trade names), DEN-431, DEN-439 (above are manufactured by The Dow Chemical Company, trade names), EOCN-120, EOCN-102S, EOCN-103S, EOCN-104S, EOCN-1012, EOCN-1025, EOCN-1027, BREN (above are manufactured by Nippon Kayaku Co., Ltd., manufactured by BASF, trade names), EPN-1138, EPN-1235, EPN-1299 (all manufactured by BASF, trade names), N-730, N-770, N-865, N-665, N-673, VH-4150, VH-4240 (all manufactured by DIC Corporation, trade names), etc.
[0060] Preferred examples of the epoxy resin (a2) include bisphenol A epoxy resins or bisphenol F epoxy resins having a structural unit represented by the following formula (IV). Examples of epoxy resins having such a structural unit include bisphenol A epoxy resins or bisphenol F epoxy resins represented by the following formula (IV').
[0061]
[0062] In formula (IV) and (IV'), R 14 Represents a hydrogen atom or a methyl group, and there are multiple R 14 Can be the same or different, Y 6 In formula (IV'), n2 represents a number greater than 1. When n2 is greater than 2, multiple Y 6 Can be the same or different, at least one Y 6 It is a glycidyl group.
[0063] From the perspective of suppressing the generation of undercuts and improving the linearity and resolution of the resist pattern profile, R 14 It can be a hydrogen atom. From the viewpoint of further improving the thermal shock resistance, Y 6 It may be a glycidyl group. n2 represents 1 or more, but may also be 10 to 100, 10 to 80, or 15 to 60. When n2 is within the above range, the linearity of the resist pattern profile, the adhesion to the copper substrate, and the heat resistance are easily improved.
[0064] Y in formula (IV) 6 For example, a bisphenol A epoxy resin or a bisphenol F epoxy resin which is a glycidyl group can be obtained by making Y in formula (IV) 6 The hydroxyl group of bisphenol A epoxy resin or bisphenol F epoxy resin is a hydrogen atom (-OY 6 ) is obtained by reacting with epichlorohydrin.
[0065] To promote the reaction between the hydroxyl group and epichlorohydrin, the reaction can be carried out in a polar organic solvent such as dimethylformamide, dimethylacetamide, or dimethyl sulfoxide in the presence of an alkali metal hydroxide at a reaction temperature of 50 to 120°C. When the reaction temperature is within this range, the reaction does not become excessively slow, and side reactions can be suppressed.
[0066] As the bisphenol A-type epoxy resin or bisphenol F-type epoxy resin represented by formula (IV'), for example, jER807, jER815, jER825, jER827, jER828, jER834, jER1001, jER1004, jER1007, jER1009 (these are manufactured by Mitsubishi Chemical Corporation, trade names), DER-330, DER-301, DER-361 (these are manufactured by The Dow Chemical Company, trade names), YD-8125, YDF-170, YDF-175S, YDF-2001, YDF-2004, YDF-8170 (these are manufactured by NIPPON STEEL Chemical & Material Co., Ltd., trade names), etc. are commercially available.
[0067] Preferred examples of the epoxy resin (a2) include trisphenolmethane epoxy resins having a structural unit represented by the following formula (V). Examples of trisphenolmethane epoxy resins having such a structural unit include trisphenolmethane epoxy resins represented by the following formula (V').
[0068]
[0069] In formula (V) and (V'), Y 7 represents a hydrogen atom or a glycidyl group, multiple Y 7 Can be the same or different, at least one Y 7 In formula (V'), n3 represents a number of 1 or greater.
[0070] From the perspective of suppressing the generation of undercuts and upper defects and improving the linearity and resolution of the resist pattern profile, Y 7 Y as a hydrogen atom in 7 With Y as glycidyl group 7 The molar ratio of Y can be 0 / 100 to 30 / 70. 7 At least one of them is a glycidyl group. n3 is 1 or more, but may be 10 to 100, 15 to 80, or 15 to 70. When n3 is within the above range, the linearity of the resist pattern profile, the adhesion to the copper substrate, and the heat resistance are easily improved.
[0071] As the trisphenol methane type epoxy resin represented by formula (V′), for example, FAE-2500, EPPN-501H, EPPN-502H (these are manufactured by Nippon Kayaku Co., Ltd., trade names) and the like are commercially available.
[0072] Preferred examples of the epoxy resin (a2) include biphenyl epoxy resins having a structural unit represented by the following formula (VI): Examples of biphenyl epoxy resins having such a structural unit include biphenyl epoxy resins represented by the following formula (VI').
[0073]
[0074] In formula (VI) and (VI'), Y 8 represents a hydrogen atom or a glycidyl group, multiple Y 8 Can be the same or different, at least one Y 8 In formula (V'), n4 represents a number of 1 or greater.
[0075] As the biphenyl type epoxy resin represented by formula (VI'), for example, NC-3000, NC-3000-L, NC-3000-H, NC-3000-FH-75M, NC-3100, CER-3000-L (all manufactured by Nippon Kayaku Co., Ltd., trade names) and the like are commercially available.
[0076] As the epoxy resin (a2), at least one selected from the group consisting of a novolac-type epoxy resin having a structural unit represented by formula (III), a bisphenol A-type epoxy resin having a structural unit represented by formula (IV), and a bisphenol F-type epoxy resin having a structural unit represented by formula (IV) is preferred, and a bisphenol F-type epoxy resin having a structural unit represented by formula (IV) is more preferred.
[0077] From the viewpoints of thermal shock resistance, warpage reduction, and resolution, a bisphenol novolac-type epoxy resin having a structural unit represented by the above formula (I) can be used as the component (a1) (A1) and a bisphenol A-type epoxy resin or a bisphenol F-type epoxy resin having a structural unit represented by the formula (IV) can be used in combination as the component (a2) (A2).
[0078] (Ethylenically unsaturated group-containing organic acid (b))
[0079] Examples of component (b) include acrylic acid; acrylic acid derivatives such as acrylic acid dimers, methacrylic acid, β-furfuryl acrylic acid, β-styryl acrylic acid, cinnamic acid, crotonic acid, and α-cyanocinnamic acid; half-ester compounds that are reaction products of hydroxyl-containing (meth)acrylates and dibasic acid anhydrides; and half-ester compounds that are reaction products of vinyl-containing monoglycidyl ethers or vinyl-containing monoglycidyl esters and dibasic acid anhydrides. Component (b) can be used alone or in combination of two or more.
[0080] The half ester compound is obtained by, for example, reacting a hydroxyl group-containing (meth)acrylate, a vinyl group-containing monoglycidyl ether, or a vinyl group-containing monoglycidyl ester with a dibasic acid anhydride.
[0081] Examples of the hydroxyl-containing (meth)acrylates, vinyl-containing monoglycidyl ethers, and vinyl-containing monoglycidyl esters include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, and glycidyl (meth)acrylate.
[0082] Examples of the dibasic acid anhydride include succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, and itaconic anhydride.
[0083] In the reaction between components (a) and (b), the reaction can be carried out at a ratio of 0.6 to 1.05 equivalents of component (b) per 1 equivalent of epoxy groups in component (a), or 0.8 to 1.0 equivalents. This reaction ratio tends to increase photosensitivity and improve the linearity of the resist pattern profile.
[0084] Component (a) and component (b) can be dissolved in an organic solvent and reacted. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, butyl cellosolve acetate, and carbitol acetate; aliphatic hydrocarbons such as octane and decane; and petroleum solvents such as petroleum ether, naphtha, hydrogenated naphtha, and solvent naphtha. The organic solvent may be used alone or in combination of two or more.
[0085] In order to promote the reaction of component (a) and component (b), a catalyst can be used. Examples of the catalyst include triethylamine, benzylmethylamine, methyltriethylammonium chloride, benzyltrimethylammonium chloride, benzyltrimethylammonium bromide, benzyltrimethylammonium iodide, and triphenylphosphine. The catalyst can be used alone or in combination of two or more.
[0086] From the viewpoint of promoting the reaction between components (a) and (b), the catalyst may be used in an amount of 0.01 to 10 parts by mass, 0.05 to 2 parts by mass, or 0.1 to 1 part by mass relative to 100 parts by mass of the total of components (a) and (b).
[0087] In the reaction of component (a) and component (b), a polymerization inhibitor may be used to prevent polymerization during the reaction. As the polymerization inhibitor, for example, hydroquinone, methyl hydroquinone, hydroquinone monomethyl ether, catechol and pyrogallol may be mentioned. One polymerization inhibitor may be used alone or in combination of two or more. From the viewpoint of improving stability, the amount of the polymerization inhibitor used may be 0.01 to 1 part by mass, 0.02 to 0.8 parts by mass or 0.04 to 0.5 parts by mass relative to a total of 100 parts by mass of component (a) and component (b).
[0088] From the viewpoint of productivity, the reaction temperature of the components (a) and (b) may be 60 to 150°C, 80 to 120°C, or 90 to 110°C.
[0089] Component (A'), formed by reacting components (a) and (b), has hydroxyl groups formed by a ring-opening addition reaction between the epoxy groups of component (a) and the carboxyl groups of component (b). By further reacting component (c) with component (A'), an acid-modified vinyl-containing epoxy resin can be obtained in which the hydroxyl groups of component (A') (including those originally present in component (a)) and the acid anhydride groups of component (c) are half-esterified.
[0090] (Polyacid anhydride (c))
[0091] Examples of the component (c) include succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, and itaconic anhydride. From the perspective of resolution, the component (c) may be tetrahydrophthalic anhydride. The components (c) may be used alone or in combination of two or more.
[0092] The reaction temperature of the component (A') and the component (c) may be 50 to 150°C, 60 to 120°C, or 70 to 100°C from the viewpoint of productivity.
[0093] If necessary, as the component (a), for example, a hydrogenated bisphenol A epoxy resin or a styrene-maleic acid resin such as a hydroxyethyl (meth)acrylate-modified styrene-maleic anhydride copolymer may be used in combination.
[0094] In the reaction between the components (A') and (c), for example, the acid value of the component (A) can be adjusted by reacting the component (c) in an amount of 0.1 to 1.0 equivalents per equivalent of hydroxyl groups in the component (A').
[0095] The acid value of component (A) can be 30 to 150 mgKOH / g, 40 to 120 mgKOH / g, or 50 to 100 mgKOH / g. If the acid value of component (A) is 30 mgKOH / g or greater, the photosensitive resin composition tends to have excellent solubility in a dilute alkaline solution. If the acid value of component (A) is 150 mgKOH / g or less, the electrical properties of the permanent resist tend to be improved.
[0096] The weight average molecular weight (Mw) of the component (A) is not particularly limited. From the viewpoints of resolution, adhesion, heat resistance, and electrical insulation, the Mw of the component (A) may be 3,000 to 30,000, 4,000 to 25,000, or 5,000 to 18,000.
[0097] Mw can be measured by gel permeation chromatography (GPC). Mw is measured, for example, under the following GPC conditions, and the value converted using a calibration curve of standard polystyrene can be set as Mw. The calibration curve can be prepared using a set of five samples ("PStQuick MP-H" and "PStQuick B", manufactured by Tosoh Corporation) as standard polystyrene.
[0098] GPC apparatus: High-speed GPC apparatus "HCL-8320GPC" (manufactured by Tosoh Corporation)
[0099] Detector: Differential refractometer or UV detector (manufactured by Tosoh Corporation)
[0100] Column: TSKgel SuperMultipore HZH (column length: 15 cm, column inner diameter: 4.6 mm) (manufactured by Tosoh Corporation)
[0101] Eluent: tetrahydrofuran (THF)
[0102] Measurement temperature: 40℃
[0103] Flow rate: 0.35mL / min
[0104] Sample concentration: 10 mg / THF5 mL
[0105] Injection volume: 20 μL
[0106] From the viewpoint of improving the heat resistance, electrical properties, and chemical resistance of the permanent resist, the content of component (A) in the photosensitive resin composition may be 20 to 80 mass %, 25 to 70 mass %, or 3 to 50 mass %, based on the total solid content of the photosensitive resin composition.
[0107] When components (A1) and (A2) are used in combination as component (A), the total content of components (A1) and (A2) in component (A) may be 80 to 100 mass%, 90 to 100 mass%, 95 to 100 mass%, or 100 mass%, based on the total amount of component (A). Even when component (A1) or (A2) is used alone, the content can be appropriately selected from the above ranges.
[0108] When components (A1) and (A2) are used in combination as component (A), the mass ratio (A1 / A2) may be 20 / 80 to 90 / 10, 30 / 70 to 80 / 20, 40 / 60 to 75 / 25, or 50 / 50 to 70 / 30 from the viewpoint of linearity of the resist pattern profile, electroless plating resistance, and heat resistance.
[0109] <Component (B): Photopolymerizable compound>
[0110] The photosensitive resin composition of this embodiment contains a photopolymerizable compound as component (B). Component (B) is not particularly limited as long as it is a compound having a functional group exhibiting photopolymerization. Examples of functional groups exhibiting photopolymerization include groups having ethylenically unsaturated bonds such as vinyl, allyl, propargyl, butenyl, ethynyl, phenylethynyl, maleimide, nadicimide, and (meth)acryloyl groups. From the perspective of reactivity, component (B) may contain a compound having a (meth)acryloyl group.
[0111] Examples of the component (B) include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate; mono- or di-(meth)acrylates of glycols such as ethylene glycol, methoxytetraethylene glycol, and polyethylene glycol; (meth)acrylamide compounds such as N,N-dimethyl(meth)acrylamide and N-hydroxymethyl(meth)acrylamide; aminoalkyl (meth)acrylates such as N,N-dimethylaminoethyl(meth)acrylate; hexanediol, trimethylolpropane, pentaerythritol, ditrihydroxypropane, and the like. Polyvalent (meth)acrylates of polyols such as methylpropane, dipentaerythritol, and tris-hydroxyethyl isocyanurate, or their ethylene oxide or propylene oxide adducts; (meth)acrylate compounds of ethylene oxide or propylene oxide adducts of phenol compounds such as phenoxyethyl (meth)acrylate and polyethoxydi(meth)acrylate of bisphenol A; (meth)acrylates of glycidyl ethers such as glycerol diglycidyl ether, trimethylolpropane triglycidyl ether, and triglycidyl isocyanurate; and melamine (meth)acrylate. Component (B) can be used alone or in combination of two or more.
[0112] The content of component (B) can be 0.1 to 15% by mass, 0.1 to 10% by mass, 0.5 to 8% by mass, or 2 to 7% by mass, based on the total solid content in the photosensitive resin composition. If the content of component (B) is 0.1% by mass or more, the exposed portion is less likely to dissolve during development, while if it is 15% by mass or less, heat resistance is easily improved.
[0113] <Component (C): Photopolymerization Initiator>
[0114] The photosensitive resin composition of this embodiment contains a photopolymerization initiator as component (C). Component (C) is not particularly limited as long as it can polymerize the photopolymerizable compound as component (B). Component (C) can be used alone or in combination of two or more.
[0115] Examples of the component (C) include benzoin compounds such as benzoin, benzoin methyl ether, and benzoin isopropyl ether; acetophenone compounds such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexylphenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propane, and N,N-dimethylaminoacetophenone; and 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butyl Anthraquinone compounds such as 1-aminoanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, and 2-aminoanthraquinone; thioxanthone compounds such as 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; ketal compounds such as acetophenone dimethyl ketal and benzyl dimethyl ketal; benzophenone compounds such as benzophenone, methyl benzophenone, 4,4'-dichlorobenzophenone, 4,4'-bis(diethylamino)benzophenone (Michler's ketone), and 4-benzoyl-4'-methyldiphenyl sulfide; 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer imidazole compounds such as imidazole dimer, 2-(o-chlorophenyl)-4,5-di(m-methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer, 2,4-di(p-methoxyphenyl)-5-phenylimidazole dimer, 2-(2,4-dimethoxyphenyl)-4,5-diphenylimidazole dimer; acridine compounds such as 9-phenylacridine and 1,7-bis(9,9'-acridinyl)heptane; 2,4 ,6-trimethylbenzoyldiphenylphosphine oxide and other acylphosphine oxide compounds; oxime ester compounds such as 1,2-octanedione-1-[4-(phenylthio)phenyl]-2-(O-benzoyl oxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyl oxime), and 1-phenyl-1,2-propanedione-2-[O-(ethoxycarbonyl)oxime]; and tertiary amine compounds such as N,N-dimethylaminobenzoic acid ethyl ester, N,N-dimethylaminobenzoic acid isopentyl ester, 4-dimethylaminobenzoic acid pentyl ester, triethylamine, and triethanolamine.
[0116] The component (C) preferably contains at least one selected from the group consisting of an acetophenone compound, a thioxanthone compound, a benzophenone compound, an oxime ester compound, and an acylphosphine oxide compound. The component (C) can be selected based on the desired performance. From the perspective of improving the heat resistance of the solder, the component (C) may contain an acetophenone compound, a thioxanthone compound, or an acylphosphine oxide compound. From the perspective of improving the curability of the bottom through photobleaching, the component (C) may contain an acylphosphine oxide compound. From the perspective of volatilization and difficulty in outgassing, the component (C) may contain an acetophenone compound.
[0117] The content of component (C) is not particularly limited and can be 0.2 to 15% by mass, 0.4 to 5% by mass, or 0.6 to 1% by mass based on the total solid content of the photosensitive resin composition. If the content of component (C) is 0.2% by mass or more, the exposed portion is less likely to dissolve during development, while if it is 15% by mass or less, a decrease in heat resistance is easily suppressed.
[0118] <Component (D): Inorganic filler>
[0119] The photosensitive resin composition of this embodiment contains an inorganic filler including a surface-treated filler as component (D). The surface-treated filler can be obtained by treating the surface of the inorganic filler with a surface treatment agent. By treating the surface of the inorganic filler, the adhesive strength at the filler interface with component (A) is improved, thereby improving the heat resistance and thermal shock resistance of the permanent resist. One surface-treated filler can be used alone or in combination of two or more.
[0120] Examples of the inorganic filler include silicon dioxide (SiO2), aluminum oxide (Al2O3), titanium dioxide (TiO2), tantalum oxide (Ta2O5), zirconium oxide (ZrO2), silicon nitride (Si3N4), barium titanate (BaO·TiO2), barium carbonate (BaCO3), magnesium carbonate (MgCO3), aluminum hydroxide (Al(OH)3), magnesium hydroxide (Mg(OH)2), lead titanate (PbO·TiO2), lead zirconate titanate (PZT), lead lanthanum zirconate titanate (PLZT), gallium oxide (Ga2O3), spinel (MgO·A l2O3), mullite (3Al2O3·2SiO2), cordierite (2MgO·2Al2O3 / 5SiO2), talc (3MgO·4SiO2·H2O), aluminum titanate (TiO2·Al2O3), yttria-containing zirconium oxide (Y2O3·ZrO2), barium silicate (BaO·8SiO2), boron nitride (BN), calcium carbonate (CaCO3), barium sulfate (BaSO4), calcium sulfate (CaSO4), zinc oxide (ZnO), magnesium titanate (MgO·TiO2), hydrotalcite, mica, calcined kaolin, and carbon (C). The inorganic filler may contain silica to improve heat resistance, barium sulfate to improve heat resistance and adhesive strength, or a combination of silica and barium sulfate.
[0121] The surface treatment agent is not particularly limited as long as it is an organic compound that coats the surface of the inorganic filler and has the effect of inhibiting the reaction between the organosilane compound as component (E) and the uncoated inorganic filler. The surface treatment agent preferably has a functional group capable of forming a bond with a functional group on the surface of the inorganic filler. For example, a functional group such as a silyl group that can form a bond with a silanol group present on the surface of silica by hydrolysis can be mentioned.
[0122] Examples of surface treatment agents include organozirconium compounds, organotitanium compounds, organoaluminum compounds, and organosilane compounds. The method for surface treating the inorganic filler is not particularly limited. For example, an organosilane compound can be used as a silane coupling agent to treat silica. Surface-treated fillers can also be purchased commercially.
[0123] Examples of the organic zirconium compound include tetrapropoxy zirconium (zirconium tetrapropoxide), tetrabutoxy zirconium (zirconium tetrabutoxide), normal propylzirconate, normal butylzirconate, and zirconium tetraacetylacetonate. Examples of the organic titanium compound include tetraethyl orthotitanate, tetra(2-ethylhexyl) orthotitanate, tetraisopropyl titanate, tetra-n-butyl titanate, and titanium acetylacetonate. Examples of the organic aluminum compound include aluminum secondary butoxide. Examples of the organic silane compound include epoxy silane compounds, aminosilane compounds, mercaptosilane compounds, (meth)acrylic silane compounds, vinyl silane compounds, alkyl silane compounds, isocyanate-containing silane compounds, isocyanurate-containing silane compounds, fluorene skeleton-containing silane compounds, and benzotriazole-containing silane compounds.
[0124] Examples of the epoxysilane compound include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.
[0125] Examples of the aminosilane compound include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-(2-aminoethyl)aminopropylmethyldimethoxysilane, 3-phenylaminopropyltrimethoxysilane, and N-(1,3-dimethylbutylene)-3-aminopropyltriethoxysilane.
[0126] Examples of the mercaptosilane compound include 3-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, and 3-mercaptopropyltriethoxysilane.
[0127] Examples of the (meth)acrylic silane compound include 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, and 3-methacryloxypropyltriethoxysilane.
[0128] Examples of the vinylsilane compound include vinyltriacetoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, allyltrimethoxysilane, diallyldimethylsilane, and p-phenylyltrimethoxysilane.
[0129] Examples of the alkylsilane compound include dimethoxydiphenylsilane. Examples of the isocyanate group-containing silane compound include tris-(trimethoxysilylpropyl)isocyanurate. Examples of the isocyanurate group-containing silane compound include 3-isocyanatepropyltriethoxysilane.
[0130] Examples of fluorene skeleton-containing silane compounds include "SC-001" and "SC-003" manufactured by Osaka Gas Chemicals Co., Ltd. Examples of benzotriazole group-containing silane compounds include "X-12-1214A" manufactured by Shin-Etsu Chemical Co., Ltd.
[0131] The elemental composition of aluminum on the surface of the inorganic filler surface-treated with an organoaluminum compound or an organosilane compound can be appropriately selected from 0.5 to 10 atomic %, 1 to 5 atomic % or 1.5 to 3.5 atomic %. The elemental composition of silicon on the surface of the inorganic filler can be appropriately selected from 0.5 to 10 atomic %, 1 to 5 atomic % or 1.5 to 3.5 atomic %. The elemental composition of carbon on the surface of the inorganic filler can be appropriately selected from 10 to 30 atomic %, 15 to 25 atomic % or 18 to 23 atomic %. Their elemental compositions can be measured using XPS (X-ray photoelectrometry).
[0132] Silica fillers surface-treated with an organoaluminum compound or an organosilane compound can also be prepared by treating ADMATECS COMPANY LIMITED's ADMAFINE silica series with the aforementioned silane compounds. Barium sulfate surface-treated with an organoaluminum compound or an organosilane compound is commercially available under the trade name "BFN40DC" manufactured by Nippon Solvay KK.
[0133] From the viewpoint of resolution, the average particle size of component (D) may be 0.01 to 5 μm, 0.05 to 3 μm, 0.1 to 2 μm, or 0.15 to 1 μm. The average particle size of component (D) is the average particle size of the component dispersed in the photosensitive resin composition and is measured by the following procedure.
[0134] After diluting the photosensitive resin composition 1000-fold with a solvent (methyl ethyl ketone), the particle size distribution of the particles dispersed in the solvent was measured using a submicron particle analyzer (manufactured by Beckman Coulter, Inc., trade name "N5") at a refractive index of 1.38 in accordance with international standard ISO 13321. The particle size at the 50% cumulative value (volume basis) of the particle size distribution was taken as the average particle size. The same procedure can be used to measure component (D) contained in a photosensitive layer formed using the photosensitive resin composition and its cured film.
[0135] The content of the surface treatment filler is not particularly limited, but may be 15-70% by mass, 20-65% by mass, 25-60% by mass, 25-50% by mass, or 25-45% by mass based on the total solid content of the photosensitive resin composition. When the content of the surface treatment filler is within the above range, the permanent resist tends to have excellent strength, heat resistance, resolution, etc.
[0136] <Component (E): Organosilane compound>
[0137] The photosensitive resin composition of the present embodiment is not particularly limited as the component (E), and a known and commonly used organosilane compound can be used. The organosilane compound can be used alone or in combination of two or more.
[0138] Examples of the organic silane compound include epoxy silane compounds, amino silane compounds, mercapto silane compounds, (meth)acrylic silane compounds, vinyl silane compounds, alkyl silane compounds, isocyanate group-containing silane compounds, isocyanurate group-containing silane compounds, fluorene skeleton-containing silane compounds, and benzotriazole group-containing silane compounds.
[0139] The component (E) can be selected from the organosilane compounds exemplified as the surface treatment agent for the component (D). In particular, the component (E) may include a silane compound containing a benzotriazole group from the perspective of adhesion to the copper substrate, or a silane compound containing a fluorene skeleton from the perspective of heat resistance.
[0140] The content of the (E) component is not particularly limited. Relative to 100 parts by mass of the content of the (D) component, the content of the (E) component may be 1 to 50 parts by mass, 1 to 25 parts by mass, 1.5 to 25 parts by mass, 2 to 20 parts by mass, or 2 to 15 parts by mass. If the content of the (E) component is within the above range, the permanent resist has excellent thermal shock resistance and maintains good developability, adhesion, and heat resistance. In addition, from the viewpoint of further improving the thermal shock resistance and heat resistance of the permanent resist, the content of the (E) component may be 1 to 40 parts by mass, 1.5 to 30 parts by mass, 2 to 25 parts by mass, or 2.5 to 20 parts by mass relative to 100 parts by mass of the (A) component. Based on the total solid content of the photosensitive resin composition, the content of the (E) component may be 0.5 to 10% by mass, 0.8 to 9% by mass, 1 to 8% by mass, or 1.2 to 7% by mass.
[0141] <(F) Ingredient: Pigment>
[0142] From the perspective of improving the appearance of concealing conductor patterns, the photosensitive resin composition of this embodiment may further contain a pigment as component (F). Component (F) may be a colorant that develops a desired color when concealing wiring (conductor patterns), etc. Component (F) may be used alone or in combination of two or more.
[0143] Examples of the component (F) include phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, carbon black, and naphthalene black.
[0144] From the viewpoint of facilitating identification of the manufacturing apparatus and further concealing wiring, the content of the component (F) may be 0.01 to 5.0 mass %, 0.03 to 3.0 mass %, or 0.05 to 2.0 mass % based on the total solid content in the photosensitive resin composition.
[0145] <(G) Component: Curing Agent>
[0146] The photosensitive resin composition of this embodiment may further comprise a curing agent as component (G). Component (G) includes, for example, compounds that cure by heat, ultraviolet light, or the like, or compounds that cure by reaction with the carboxyl or hydroxyl groups of component (A) by heat, ultraviolet light, or the like. The use of a curing agent can improve the heat resistance, adhesion, and chemical resistance of the permanent resist.
[0147] Examples of the component (G) include thermosetting compounds such as epoxy compounds, blocked isocyanates, melamine compounds, and oxazoline compounds. Examples of the melamine compound include triaminotriazine, hexamethoxymelamine, and hexabutoxylated melamine. The component (G) may be used alone or in combination of two or more.
[0148] As the epoxy compound, for example, the compounds listed as component (a) can be used. The epoxy compound can be liquid or solid at room temperature (25°C). As the epoxy compound, for example, bisphenol A epoxy resin, bisphenol F epoxy resin, hydrogenated bisphenol A epoxy resin, brominated bisphenol A epoxy resin, novolac epoxy resin, bisphenol S epoxy resin, biphenyl epoxy resin, naphthalene epoxy resin, dicyclic epoxy resin, hydantoin epoxy resin, triglycidyl isocyanurate and dixylenol epoxy resin can be mentioned. Component (G) can contain at least one selected from the group consisting of bisphenol-type epoxy resins such as bisphenol A epoxy resin and bisphenol F epoxy resin and novolac epoxy resin.
[0149] As blocked isocyanates, addition reaction products of polyisocyanate compounds and isocyanate blocking agents are used. Examples of melamine compounds include triaminotriazine, hexamethoxymelamine, and hexabutoxylated melamine. Among these, epoxy compounds (epoxy resins) are preferred from the viewpoint of further improving the heat resistance of the cured film.
[0150] The content of component (G) can be 2-40% by mass, 3-30% by mass, or 5-20% by mass based on the total solid content of the photosensitive resin composition. When the content of component (G) is within the above range, better developability can be maintained and the heat resistance of the resulting permanent resist can be further improved.
[0151] When an epoxy compound is used as the component (G), a curing accelerator for epoxy resin may be used in combination in order to further improve various properties of the permanent resist, such as heat resistance, adhesion, and chemical resistance.
[0152] Examples of curing accelerators include imidazole derivatives such as 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 2-phenylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole; guanamines such as acetoguanamine and benzoguanamine; polyamines such as diaminodiphenylmethane, m-phenylenediamine, m-xylenediamine, diaminodiphenylsulfone, dicyandiamide, urea, urea derivatives, melamine, and polyhydrazides; organic acid salts or epoxy adducts thereof; amine complexes of boron trifluoride; and triazine derivatives such as ethyldiamino-s-triazine, 2,4-diamino-s-triazine, and 2,4-diamino-6-xylyl-s-triazine. From the perspective of improving reliability, the content of the curing accelerator can be 0.01 to 30% by mass or 0.1 to 20% by mass based on the total solids content of the photosensitive resin composition.
[0153] <(H) Component: Elastomer>
[0154] The photosensitive resin composition of this embodiment may further contain an elastomer as component (H). By adding component (H) to the photosensitive resin composition, it is possible to suppress the reduction in flexibility and adhesive strength caused by deformation (internal stress) within the resin due to cure shrinkage of component (A). In other words, the flexibility and adhesive strength of the permanent resist formed from the photosensitive resin composition can be improved.
[0155] Examples of the component (H) include styrene elastomers, olefin elastomers, urethane elastomers, polyester elastomers, polyamide elastomers, acrylic elastomers, and silicone elastomers. Thermoplastic elastomers are composed of a hard segment component that contributes to heat resistance and strength, and a soft segment component that contributes to flexibility and toughness. The component (H) can be used alone or in combination of two or more.
[0156] Examples of styrene-based elastomers include styrene-butadiene-styrene block copolymers, styrene-isoprene-styrene block copolymers, styrene-ethylene-butylene-styrene block copolymers, and styrene-ethylene-propylene-styrene block copolymers. As components constituting styrene-based elastomers, in addition to styrene, styrene derivatives such as α-methylstyrene, 3-methylstyrene, 4-propylstyrene, and 4-cyclohexylstyrene can also be used.
[0157] Examples of the olefin-based elastomer include ethylene-propylene copolymers, ethylene-α-olefin copolymers, ethylene-α-olefin-non-conjugated diene copolymers, propylene-α-olefin copolymers, butene-α-olefin copolymers, ethylene-propylene-diene copolymers, copolymers of non-conjugated dienes such as dicyclopentadiene, 1,4-hexadiene, cyclooctadiene, methylene norbornene, ethylidene norbornene, butadiene, and isoprene with α-olefins, epoxy-modified polybutadiene, and carboxylic acid-modified butadiene-acrylonitrile copolymers.
[0158] The epoxy-modified polybutadiene preferably has a hydroxyl group at a molecular terminal, more preferably at both molecular terminals, and even more preferably only at both molecular terminals. The number of hydroxyl groups in the epoxy-modified polybutadiene may be one or more, preferably 1 to 5, more preferably 1 or 2, and even more preferably 2.
[0159] As urethane elastomers, compounds composed of a hard segment formed from a low-molecular-weight (short-chain) diol and a diisocyanate, and a soft segment formed from a high-molecular-weight (long-chain) diol and a diisocyanate can be used. Examples of low-molecular-weight diols include ethylene glycol, propylene glycol, 1,4-butanediol, and bisphenol A. Examples of the high molecular weight diol include polypropylene glycol, polytetramethylene oxide, poly(1,4-butylene adipate), poly(ethylene-1,4-butylene adipate), polycaprolactone, poly(1,6-hexylene carbonate), and poly(1,6-hexylene-neopentylene adipate).
[0160] The number average molecular weight (Mn) of the low molecular weight diol may be 48 to 500. The Mn of the high molecular weight diol may be 500 to 10000. As urethane elastomers, for example, PANDEX T-2185 and T-2983N (manufactured by DIC Corporation) and Miractran E790 (manufactured by Nippon Miractran Company Limited) are commercially available.
[0161] As polyester elastomers, compounds obtained by polycondensing a dicarboxylic acid or a derivative thereof with a diol compound or a derivative thereof can be used. Examples of dicarboxylic acids include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, and naphthalene dicarboxylic acid, and aromatic dicarboxylic acids in which aromatic hydrogen atoms are substituted with methyl, ethyl, phenyl, or the like; aliphatic dicarboxylic acids having 2 to 20 carbon atoms such as adipic acid, sebacic acid, and dodecanedicarboxylic acid; and alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid.
[0162] Examples of the diol compound include aliphatic diols such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, and 1,10-decanediol; alicyclic diols such as 1,4-cyclohexanediol; and aromatic diols such as bisphenol A, bis-(4-hydroxyphenyl)methane, bis-(4-hydroxy-3-methylphenyl)propane, and resorcinol.
[0163] As polyester elastomers, multi-block copolymers containing an aromatic polyester (e.g., polybutylene terephthalate) as a hard segment component and an aliphatic polyester (e.g., polytetramethylene glycol) as a soft segment component can be used. Polyester elastomers are available in different grades depending on the type, ratio, and molecular weight of the hard and soft segments. Examples of commercially available polyester elastomers include Hytrel (manufactured by Toray Celanese Co., Ltd., "Hytrel" is a registered trademark), Pelprene (manufactured by Toyobo Co., Ltd., "Pelprene" is a registered trademark), and Espel (manufactured by Showa Denko Materials Co., Ltd., "Espel" is a registered trademark).
[0164] Acrylic elastomers can use compounds containing acrylate-based structural units as the main component. Examples of acrylates include ethyl acrylate, butyl acrylate, methoxyethyl acrylate, and ethoxyethyl acrylate. Acrylic elastomers can be compounds formed by copolymerizing acrylates with acrylonitrile, or compounds formed by further copolymerizing monomers having functional groups that serve as crosslinking points. Examples of monomers having functional groups include glycidyl methacrylate and allyl glycidyl ether. Examples of acrylic elastomers include acrylonitrile-butyl acrylate copolymers, acrylonitrile-butyl acrylate-ethyl acrylate copolymers, and acrylonitrile-butyl acrylate-glycidyl methacrylate copolymers.
[0165] Polyamide-based elastomers are broadly classified into two types: polyether block amide type, which uses polyamide in the hard segment and polyether or polyester in the soft segment, and polyetherester block amide type. Examples of polyamides include polyamide-6, polyamide-11, and polyamide-12. Examples of polyethers include polyoxyethylene glycol, polyoxypropylene glycol, and polytetramethylene glycol.
[0166] Silicone elastomers are compounds primarily composed of organopolysiloxanes. Examples of organopolysiloxanes include polydimethylsiloxane, polymethylphenylsiloxane, and polydiphenylsiloxane. Silicone elastomers can also be compounds obtained by modifying a portion of an organopolysiloxane with a vinyl group, an alkoxy group, or the like.
[0167] The content of component (H) can be 1 to 40 parts by mass, 4 to 30 parts by mass, 5 to 25 parts by mass, or 10 to 20 parts by mass relative to 100 parts by mass of component (A). By setting the content of component (H) within the above range, the unexposed areas of the photosensitive layer are more easily eluted in the developer, and the elastic modulus of the permanent resist in high temperature regions tends to be further reduced.
[0168] <Other ingredients>
[0169] The photosensitive resin composition of this embodiment may contain a diluent such as an organic solvent, as needed, to adjust the viscosity. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, butyl cellosolve acetate, and carbitol acetate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, naphtha, hydrogenated naphtha, and solvent naphtha.
[0170] When a diluent is used, the content of the diluent in the photosensitive resin composition may be 10-50 mass %, 20-40 mass %, or 25-35 mass %. By setting the diluent content within the above range, the coating properties of the photosensitive resin composition can be improved, and a higher-definition pattern can be formed.
[0171] The photosensitive resin composition of this embodiment may also contain various additives as needed. Examples of these additives include polymerization inhibitors such as hydroquinone, methylhydroquinone, hydroquinone monomethyl ether, catechol, and pyrogallol; thickeners such as bentonite and montmorillonite; defoamers such as silicone-based, fluorine-based, and vinyl-based defoamers; silane coupling agents; and flame retardants such as brominated epoxy compounds, acid-modified brominated epoxy compounds, antimony compounds, phosphorus-based phosphate compounds, aromatic condensed phosphate esters, and halogen-containing condensed phosphate esters. These additives may be used alone or in combination.
[0172] The photosensitive resin composition of the present embodiment can be prepared by uniformly mixing the above-mentioned components using a roll mill, a bead mill, or the like.
[0173] [Photosensitive element]
[0174] The photosensitive element of this embodiment includes a support film and a photosensitive layer containing the above-mentioned photosensitive resin composition. Figure 1 : is a cross-sectional view schematically showing a photosensitive element of this embodiment. Figure 1 As shown, the photosensitive element 1 includes a support film 10 and a photosensitive layer 20 formed on the support film 10 .
[0175] The photosensitive element 1 can be produced by, for example, coating the photosensitive resin composition of this embodiment on the support film 10 by a known method such as reverse roll coating, gravure roll coating, comma coating, or curtain coating, and then drying the coating to form the photosensitive layer 20 .
[0176] Examples of the support film include polyester films such as polyethylene terephthalate and polybutylene terephthalate, and polyolefin films such as polypropylene and polyethylene. The thickness of the support film can be, for example, 5 to 100 μm. The thickness of the photosensitive layer can be, for example, 10 to 50 μm, 15 to 40 μm, or 20 to 30 μm.
[0177] The coating film can be dried using hot air drying, far infrared radiation, or near infrared radiation. The drying temperature can be 60-120°C, 70-110°C, or 80-100°C. The drying time can be 1-60 minutes, 2-30 minutes, or 5-20 minutes.
[0178] A protective film 30 covering the photosensitive layer 20 may be further provided on the photosensitive layer 20. The photosensitive element 1 may also have the protective film 30 laminated on the surface of the photosensitive layer 20 opposite to the surface in contact with the support film 10. For example, a polymer film such as polyethylene or polypropylene may be used as the protective film 30. The protective film may be the same film as the support film or a different film therefrom.
[0179] [Printed circuit board]
[0180] The printed wiring board of this embodiment includes a permanent resist containing a cured product of the photosensitive resin composition of this embodiment. The printed wiring board of this embodiment includes a permanent resist containing a cured product of the photosensitive resin composition of this embodiment, and thus can reduce the occurrence of cracks in the permanent resist.
[0181] The method for manufacturing a printed wiring board according to this embodiment comprises forming a photosensitive layer on a substrate using the aforementioned photosensitive resin composition or the aforementioned photosensitive element, exposing and developing the photosensitive layer to form a resist pattern, and curing the resist pattern to form a permanent resist. An example of each step is described below.
[0182] First, a metal-clad laminate such as a copper-clad laminate is prepared as a substrate, and a photosensitive layer is formed on the substrate. When using a photosensitive resin composition, the photosensitive resin composition can be applied to the substrate by screen printing, spraying, roller coating, curtain coating, electrostatic coating, or other methods, and the resulting coating can be dried at 60-110°C to form the photosensitive layer. The coating thickness can be 10-200 μm, 15-150 μm, 20-100 μm, or 23-50 μm. When using a photosensitive element, the photosensitive layer can be formed by heat-laminating the photosensitive element onto the substrate using a laminator.
[0183] Next, the negative mask is brought into direct contact with the photosensitive layer or into contact with the photosensitive layer via a transparent film such as a support film, and after exposure to active light, the unexposed portion is dissolved and removed with a developer to form a resist pattern. As active light, for example, electron beams, ultraviolet rays, X-rays, etc. can be cited, preferably ultraviolet rays. As light sources, low-pressure mercury lamps, high-pressure mercury lamps, ultrahigh-pressure mercury lamps, halogen lamps, etc. can be used. The exposure amount can be 10 to 2000 mJ / cm 2 100~1500mJ / cm 2 or 300~1000mJ / cm 2 As a developing method, for example, an immersion method and a spraying method can be mentioned. As a developing solution, for example, an alkaline aqueous solution such as potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, or tetramethylammonium hydroxide can be used.
[0184] Then, the formed resist pattern can be subjected to at least one of post-exposure and post-heating to fully cure it and form a permanent resist. The exposure dose of the post-exposure can be 100 to 5000 mJ / cm 2 500~2000mJ / cm 2 or 700~1500mJ / cm 2 The post-heating temperature can be 100-200°C, 120-180°C, or 135-165°C. The post-heating time can be 5 minutes to 12 hours, 10 minutes to 6 hours, or 30 minutes to 2 hours. The thickness of the permanent resist can be 10-50 μm, 15-40 μm, or 20-30 μm. Afterwards, circuits are formed by etching to produce a printed circuit board.
[0185] The permanent resist of the present embodiment can be used as an interlayer insulating layer or a surface protective layer of a semiconductor element. A semiconductor element having an interlayer insulating layer or a surface protective layer formed by a cured film of the above-mentioned photosensitive resin composition, or an electronic device comprising the semiconductor element can be produced. The semiconductor element can be, for example, a memory (memory), a package, etc. having a multi-layer wiring structure, a redistribution structure, etc. As an electronic device, for example, a mobile phone, a smart phone, a tablet terminal, a personal computer, and a hard disk suspension can be cited. By having a patterned cured film formed by the photosensitive resin composition of the present embodiment, a semiconductor element and an electronic device with excellent reliability can be provided.
[0186] Example
[0187] Hereinafter, the present invention will be described in further detail with reference to Examples, but the present invention is not limited to these Examples.
[0188] (Synthesis example 1)
[0189] A bisphenol F novolac epoxy resin (manufactured by DIC Corporation, trade name "EXA-7376") having Y in formula (II) was placed in a flask equipped with a stirrer, a reflux condenser, and a thermometer. 3 and Y 4 is a glycidyl group, R 12 350 parts by mass of a bisphenol F novolac-type epoxy resin (having a structure with hydrogen atoms, epoxy equivalent: 186 g / eq), 70 parts by mass of acrylic acid, 0.5 parts by mass of methylhydroquinone, and 120 parts by mass of carbitol acetate were reacted at 90°C while stirring to completely dissolve the mixture. The resulting solution was then cooled to 60°C, 2 parts by mass of triphenylphosphine was added, and the mixture was reacted at 100°C until the acid value of the solution reached 1 mgKOH / g or less. 98 parts by mass of tetrahydrophthalic anhydride (THPAC) and 85 parts by mass of carbitol acetate were added to the reacted solution, and the reaction was continued at 80°C for 6 hours. The reaction solution was then cooled to room temperature (25°C) to obtain a solution of THPAC-modified bisphenol F novolac-type epoxy acrylate (A-1) (solids concentration: 73% by mass) as component (A1).
[0190] (Synthesis example 2)
[0191] In a flask equipped with a stirrer, a reflux condenser and a thermometer, a bisphenol F type epoxy resin (having Y in formula (IV)) was charged. 6 is a hydrogen atom, R 14 1052 parts by mass of a bisphenol F-type epoxy resin (having a structure with hydrogen atoms, epoxy equivalent: 526), 144 parts by mass of acrylic acid, 1 part by mass of methylhydroquinone, 850 parts by mass of carbitol acetate, and 100 parts by mass of solvent naphtha were reacted at 70°C while stirring to completely dissolve the mixture. The resulting solution was then cooled to 50°C, and 2 parts by mass of triphenylphosphine and 75 parts by mass of solvent naphtha were added. The mixture was then reacted at 100°C until the acid value of the solution reached 1 mgKOH / g or less. To the reacted solution were added 745 parts by mass of THPAC, 75 parts by mass of carbitol acetate, and 75 parts by mass of solvent naphtha, and the mixture was reacted at 80°C for 6 hours. The reaction solution was then cooled to room temperature (25°C) to obtain a solution of THPAC-modified bisphenol F-type epoxy acrylate (A-2) (solids concentration: 62% by mass), component (A2).
[0192] The following materials were prepared as components (B) to (H).
[0193] B-1: DPHA, dipentaerythritol hexaacrylate (manufactured by Nippon Kayaku Co., Ltd.)
[0194] C-1: 2-Methyl-[4-(methylthio)phenyl]morpholino-1-propanone (manufactured by IGM Resins BV, trade name "Ominirad 907")
[0195] C-2: 2,4-diethylthioxanthone (manufactured by Nippon Kayaku Co., Ltd., trade name "DETX-S")
[0196] C-3: 4,4'-bis(diethylamino)benzophenone (manufactured by Hodogaya Chemical Co., Ltd.)
[0197] C-4: 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone-1-(O-acetoxime) (manufactured by BASF Japan Ltd., trade name "Irgacure OXE02")
[0198] D-1: Surface-treated silica filler (silica filler (manufactured by ADMATECHS COMPANY LIMITED, trade name "SO-C2", average particle size: 0.5 μm) surface-treated with a vinylsilane compound)
[0199] D-2: Surface-treated barium sulfate (manufactured by NIPPON SOLVAY KK, trade name "BFN40DC", average particle size: 0.6 μm)
[0200] D-3: Surface-treated silica filler (a silica filler (manufactured by Denka Company Limited, trade name "SFP-20", average particle size: 0.4 μm) coated with tetrapropoxyzirconium (manufactured by Tokyo Chemical Industry Co., Ltd.))
[0201] D-4: Untreated silica filler (manufactured by Denka Company Limited, trade name "SFP-20", average particle size: 0.4 μm)
[0202] E-1: 3-glycidyloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KBM-1003")
[0203] E-2: Fluorene skeleton-containing silane compound (manufactured by Osaka Gas Chemicals Co., Ltd., trade name "SC-001")
[0204] E-3: Benzotriazole-containing silane compound (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "X-12-1241A")
[0205] E-4: Tetrapropoxide zirconium (manufactured by Tokyo Chemical Industry Co., Ltd.)
[0206] E-5: Tetraethyl orthotitanate (manufactured by Tokyo Chemical Industry Co., Ltd.)
[0207] F-1: Phthalocyanine pigment (manufactured by Sanyo Color Works, Ltd.)
[0208] G-1: Novolac-type multifunctional epoxy resin (manufactured by Nippon Kayaku Co., Ltd., trade name "RE-306")
[0209] G-2: Bisphenol A epoxy resin (manufactured by Mitsubishi Chemical Corporation, trade name "jER828")
[0210] H-1: Epoxy-modified polybutadiene (manufactured by Daicel Corporation, trade name "PB-3600")
[0211] H-2: Polyester elastomer (manufactured by Toray Celanese Co., Ltd., trade name "Hytrel 4057N")
[0212] [Photosensitive resin composition]
[0213] The components were blended in the amounts (parts by mass, based on solid content) shown in Table 1, Table 2, or Table 3 and kneaded using a three-roll mill. Carbitol acetate was then added to a solid content concentration of 70% by mass to obtain a photosensitive resin composition.
[0214] [Photosensitive element]
[0215] A 25 μm thick polyethylene terephthalate film (manufactured by TOYOBO FILMSOLUTIONS LIMITED, trade name "G2-25") was prepared as a support film. A solution prepared by adding methyl ethyl ketone to a photosensitive resin composition and diluting it was applied to the support film to a thickness of 25 μm after drying. The film was then dried at 75°C for 30 minutes using a hot air convection dryer to form a photosensitive layer. Next, a polyethylene film (manufactured by TAMAPOLY CO., LTD., trade name "NF-15") was laminated as a protective film on the surface of the photosensitive layer opposite to the side in contact with the support film to obtain a photosensitive element.
[0216] (resolution)
[0217] A 0.6 mm thick copper-clad laminate (Showa Denko Materials Co., Ltd., trade name "MCL-E-67") was prepared. While peeling and removing the protective film from the photosensitive element, a photosensitive layer was laminated onto the copper-clad laminate using a press-type vacuum laminator (Meiki Co., Ltd., trade name "MVLP-500") at a pressure of 0.4 MPa, a hot plate temperature of 80°C, a vacuuming time of 25 seconds, and a lamination pressing time of 25 seconds to obtain a laminate. Next, a negative mask having an opening pattern of a predetermined size (opening diameter size: 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 150, 200 μm) was placed in close contact with the support film of the above-mentioned laminate, and the photosensitive layer was exposed using an ultraviolet exposure device (manufactured by OAK Co., Ltd., trade name "EXM-1201") at an exposure dose that reached a complete curing level of 13 on a step tablet (manufactured by Showa Denko Materials Co., Ltd.). Thereafter, the support film was peeled off from the photosensitive layer, and a 1% by mass sodium carbonate aqueous solution was used to expose the photosensitive layer at a temperature of 1.765×10 5 The developed photosensitive layer was sprayed with a pressure of 1.5 Pa for 60 seconds to dissolve and develop the unexposed part. Then, an ultraviolet exposure device was used to expose the developed photosensitive layer at 2000 mJ / cm 2 After exposure to an exposure dose of 1000 nm, the copper-clad laminate substrate was heated at 170° C. for 1 hour to prepare a test piece having a cured film with an opening pattern of a predetermined size formed thereon. The test piece was observed using an optical microscope and evaluated according to the following criteria.
[0218] A: The minimum opening size is 30 μm or less.
[0219] B: The minimum opening size is more than 30 μm and 50 μm or less.
[0220] C: The minimum opening size exceeds 50 μm.
[0221] (Resist Pattern Shape)
[0222] The test piece was cast with an embedding resin ("jER828," manufactured by Mitsubishi Chemical Corporation, trade name, and triethylenetetramine as a curing agent) and fully cured. The specimen was then polished using a grinder ("Refine Polisher," manufactured by Refine Tec Ltd.). A cross section of the opening pattern of the cured film was cut out. The resulting cross section of the opening pattern was observed using a metallographic microscope and evaluated according to the following criteria.
[0223] A: No undercut or missing of the resist upper portion was observed, and the linearity of the pattern profile was good.
[0224] B: Undercut or missing of the upper portion of the resist or poor linearity of the pattern profile was observed.
[0225] (Thermal shock resistance)
[0226] The test pieces produced for the resolution evaluation were subjected to a temperature cycle test with one cycle consisting of 30 minutes at -65°C and 30 minutes at 150°C. The test pieces were observed visually and under an optical microscope at 1000, 2000, and 3000 cycles, and evaluated according to the following criteria.
[0227] S: No cracking was observed in 3000 cycles.
[0228] A: No cracking was observed in 2000 cycles, but cracking was observed in 3000 cycles.
[0229] B: No cracks were observed in 1000 cycles, but cracks were observed in 2000 cycles.
[0230] C: Generation of cracks was observed in 1000 cycles.
[0231] (Heat resistance)
[0232] The test pieces produced for the evaluation of resolution were placed in an environment at 150° C., and after 1000 hours and 2000 hours, the test pieces were observed visually and with an optical microscope, and evaluated according to the following criteria.
[0233] A: No cracks were observed within 2000 hours.
[0234] B: No crack generation was observed within 1000 hours, but crack generation was observed within 2000 hours.
[0235] C: No cracking was observed within 1000 hours.
[0236] (Insulation)
[0237] For the resolution evaluation, test pieces were prepared using the same method as described in "1. Resolution Evaluation" above, except that a bismaleimide triazine substrate with comb-shaped electrodes (line / space = 10 / 10 μm) was used instead of a copper-clad laminate. The test pieces were exposed to 135°C, 85% RH, and 3.3 V, and the resistance change was measured using a migration tester (manufactured by Kusumoto Chemicals, Ltd., trade name "SIR13"). The extent of migration was then observed using an optical microscope and evaluated according to the following criteria.
[0238] A: Even after more than 200 hours, no migration occurred in the permanent mask resist and the resistance value did not drop to 10 -6 Ω or less.
[0239] B: No migration occurs in the permanent mask resist within a period of 100 hours or more and less than 200 hours, and the resistance value decreases to 10 -6 Ω or less.
[0240] C: No migration occurred in the permanent mask resist and the resistance value decreased to 10 in less than 100 hours. -6 Ω or less.
[0241] [Table 1]
[0242]
[0243] [Table 2]
[0244]
[0245] [Table 3]
[0246]
[0247] Explanation of symbols
[0248] 1-photosensitive element, 10-support film, 20-photosensitive layer, 30-protective film.
Claims
1. A photosensitive resin composition for a permanent resist, comprising: (A) an acid-modified vinyl-containing resin, (B) a photopolymerizable compound, (C) a photopolymerization initiator, (D) an inorganic filler, and (E) an organic silane compound, The (D) inorganic filler includes a surface-treated filler.
2. The photosensitive resin composition according to claim 1, wherein The surface-treated filler is an inorganic filler that has been surface-treated with at least one surface-treating agent selected from the group consisting of organic zirconium compounds, organic titanium compounds, organic aluminum compounds, and organic silane compounds.
3. The photosensitive resin composition according to claim 1, wherein The (E) organic silane compound contains at least one selected from the group consisting of epoxy silane compounds, amino silane compounds, mercapto silane compounds, (meth) acrylic silane compounds, vinyl silane compounds, alkyl silane compounds, isocyanate group-containing silane compounds, isocyanurate group-containing silane compounds, fluorene skeleton-containing silane compounds and benzotriazole group-containing silane compounds.
4. The photosensitive resin composition according to claim 1, wherein The content of the (E) organosilane compound is 1 to 40 parts by mass based on 100 parts by mass of the (A) acid-modified vinyl-containing resin.
5. The photosensitive resin composition according to claim 1, wherein The (C) photopolymerization initiator contains at least one selected from the group consisting of acetophenone compounds, thioxanthone compounds, benzophenone compounds, oxime ester compounds, and acylphosphine oxide compounds.
6. A photosensitive element comprising a support film and a photosensitive layer formed on the support film, The photosensitive layer contains the photosensitive resin composition according to any one of claims 1 to 5. 7 . A printed wiring board comprising a permanent resist comprising a cured product of the photosensitive resin composition according to claim 1 .
8. A method for manufacturing a printed circuit board, comprising: A step of forming a photosensitive layer on a substrate using the photosensitive resin composition according to any one of claims 1 to 5; A step of exposing and developing the photosensitive layer to form a resist pattern; and The process of curing the resist pattern to form a permanent resist.
9. A method for manufacturing a printed circuit board, comprising: A step of forming a photosensitive layer on a substrate using the photosensitive element according to claim 6; A step of exposing and developing the photosensitive layer to form a resist pattern; and The process of curing the resist pattern to form a permanent resist.