Negative electrode binder composition, method for producing same, negative electrode, and secondary battery
The use of a high molecular weight resin with hydroxyl and acid groups, combined with an aqueous latex resin, addresses the issues of electrode expansion and high density in lithium-ion batteries, enhancing battery performance and cycle stability across temperature ranges.
Patent Information
- Application Number
- CN202380026631.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-12
- Filing Date
- 2023-03-09
- Publication Date
- 2024-12-03
AI Technical Summary
Conventional binders in lithium-ion secondary batteries fail to effectively suppress the reduction in battery performance caused by volume expansion of novel active materials, thickening of the electrode film, and high density, leading to poor capacity retention and cycle characteristics, especially at extreme temperatures.
A negative electrode binder composition comprising a high molecular weight resin with hydroxyl and acid groups, combined with an aqueous latex resin, which provides strong peel strength and resistance to electrolyte swelling, ensuring good cycle characteristics even at high and low temperatures.
The binder composition maintains slurry stability and prevents electrode expansion, resulting in improved charge and discharge characteristics and enhanced battery performance under various temperature conditions.
Smart Images

Figure BDA0005035832330000201 
Figure BDA0005035832330000511 
Figure BDA0005035832330000521
Abstract
Description
Technical Field
[0001] The present invention relates to a negative electrode binder composition and a method for preparing the same, a negative electrode comprising the negative electrode binder composition, and a secondary battery. Background Art
[0002] As a binder (binding agent) in the negative electrode of a lithium-ion secondary battery (hereinafter, sometimes referred to as "LIB"), carboxymethyl cellulose sodium salt (CMC) as a water-soluble polymer and styrene-butadiene copolymer (SBR) as an aqueous latex resin are usually used together. The main functions of the binder include 1) the function of uniformly dispersing components such as active materials and conductive additives during the electrode manufacturing process, 2) the function of adjusting the rheology of the electrode mixture slurry, 3) the leveling function of flattening the mixture layer when the slurry is applied and dried, 4) the function of bonding the mixture components and the collector, etc. Further, as functions related to battery performance, the following can be listed: 5) the function of suppressing the expansion of the electrode caused by the volume change of the active material generated during the charge and discharge cycle, 6) the function of maintaining the bonding between the active material and the collector and ensuring electronic conductivity, 7) the function of appropriately swelling by containing an electrolyte, thereby ensuring ion conductivity, etc. LIBs are widely used as rechargeable power sources for laptop computers, mobile phones, etc., but in recent years, their use in power tools such as electric tools, automobiles, and medium and large equipment such as stationary power storage devices has expanded rapidly. As the scope of application rapidly expands, the performance required of batteries in a wider temperature range has also become more diverse, but the three performances of capacity, output, and life are mainly valued, and improvements in these performances are particularly expected.
[0003] In such a situation, various measures have been tried to meet the requirements of high performance of batteries. For example, in negative electrode materials, as a measure for high capacity, novel negative electrode active materials that replace the carbon-based active materials (such as graphite) that have been widely used in the past are being studied. As novel negative electrode active materials, tin alloys, silicon alloys, silicon oxides, etc. can be listed. Compared with carbon-based active materials, these novel negative electrode active materials have very large capacities, up to several times, and even if only a small amount is added, the negative electrode capacity can be increased. However, the problem is that the capacity retention rate of these novel negative electrode active materials in the charge and discharge cycle is poorer than that of carbon-based active materials. As a reason for this, it can be listed that the novel negative electrode active materials have a larger volume expansion and contraction associated with charge and discharge than carbon-based active materials, so the destruction of the electrode structure will cause the active material to fall off and the electronic conductivity to decrease. In addition, it can also be listed that when the SEI film formed on the surface of the active material cannot follow the volume change and is destroyed, the surface of the active material not covered by the SEI film is exposed, and the electrolyte is decomposed by the new SEI film formation reaction. The SEI film is a film mainly composed of decomposition products of the electrolyte, and is formed on the surface of the active material during the first charge. It is believed that the SEI film plays a role in intervening the insertion and extraction reaction of lithium ions, while inhibiting further decomposition reactions of the electrolyte, etc., which helps to improve the performance of the battery. If the SEI film is too thin, the decomposition reaction of the electrolyte will not stop. On the contrary, if it is too thick, the resistance becomes high, which will have an adverse effect on the life and efficiency of the battery.
[0004] As a measure to solve the above-mentioned problems caused by the volume change of the novel negative electrode active material, for example, in the following patent document 1, a method of using a high-strength aromatic polyimide as a binder to suppress the volume change of the negative electrode active material is proposed. In addition, in the following patent document 2, a method of using partially cross-linked polyacrylic acid as a binder to suppress the volume change of the negative electrode active material is proposed. Furthermore, in the following patent document 3, a method of using a copolymer of acrylic acid and polyvinyl alcohol as a binder to suppress the volume change of the negative electrode active material is proposed. However, in the binder of patent document 1, the initial charge and discharge efficiency is poor, and the capacity of the active material cannot be fully utilized. In addition, in the binders of patent documents 2 and 3, the high temperature and low temperature cycle characteristics may not be sufficient.
[0005] On the other hand, when the capacity retention rate in the discharge cycle is emphasized and high capacity is desired, the method of increasing the weight of the active material per unit area without changing the graphite-based negative electrode is used, thereby increasing the capacity in the past. In this case, it is necessary to increase the thickness of the electrode layer (thick film) and increase the electrode density (high density). When the electrode is thick filmed, the migration distance of the electrons and ions inside the electrode increases, so their migration resistance increases. In addition, when high density is achieved, the gap between the active material particles is reduced, so the flow path of the electrolyte narrows, and the migration resistance of the ions increases. The increase in resistance is the main reason for the reduction in battery performance, which leads to a reduction in capacity retention and load characteristics.
[0006] As a measure to solve the problem of thick film and high density of the above-mentioned electrode, for example, in the following patent document 4, it is proposed to set the negative electrode as 2 layers, use CMC / SBR in the lower layer, and use an acrylic adhesive with high electrolyte swelling in the upper layer. However, in the method of patent document 4, there is a disadvantage that the electrode production process is doubled. In addition, since the electrolyte swelling degree of the upper layer is large, it is worried that the cycle characteristics at high temperature will be reduced. In patent document 5, a method of using a mixed resin of a resin having an acidic functional group and a polyvinylidene fluoride skeleton as the main chain and PVDF is proposed. However, when a fluorine-based resin represented by PVDF is used as a binder, an organic solvent such as NMP is used as a solvent for slurrying, but in recent years, from the perspectives of environmental concerns, operator safety and price, it is preferably used. The solvent used for slurrying is aqueous.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2019-204786
[0010] Patent Document 2: Japanese Patent Application Publication No. 2018-029069
[0011] Patent Document 3: Japanese Patent Application Publication No. 2021-136121
[0012] Patent Document 4: Japanese Patent Application Publication No. 2018-120706
[0013] Patent Document 5: Japanese Patent Application Publication No. 2020-113442 Summary of the invention
[0014] Technical problem to be solved by the invention
[0015] As described above, the binder in the conventional LIB negative electrode is insufficient in its ability to suppress the reduction in battery performance caused by the volume expansion of the novel active material, the thickening of the electrode film, and the high density. Therefore, the technical problem of the present invention is to provide a negative electrode binder composition and a method for producing the negative electrode binder composition, which can obtain good battery performance even when a novel active material is used, the electrode film is thickened, and the electrode is high-densified, and a negative electrode and a secondary battery containing the negative electrode binder composition.
[0016] Means for solving technical problems
[0017] In order to solve these technical problems, the inventors of the present invention have conducted intensive research and found that by using an unprecedented high molecular weight resin containing hydroxyl groups and acid groups and an aqueous latex resin for the negative electrode, the expansion of the electrode is suppressed, the peel strength is strong, and good cycle characteristics are exhibited even at high and low temperatures, thereby completing the present invention.
[0018] That is, the present invention is related to the following.
[0019] [1] A negative electrode binder composition comprising a water-soluble resin (X) and an aqueous latex resin (Y), wherein the water-soluble resin (X) comprises a copolymer containing a hydroxyl group-containing monomer (a) and an acid group-containing monomer (b) as essential components, the weight average molecular weight of the copolymer when measured using an aqueous GPC measuring device is 700,000 or more, and the swelling rate of a dry film of the copolymer after being immersed in a carbonate-based mixed solvent (EC (ethylene carbonate) / DEC (diethylene carbonate) = 50 / 50 (wt)) at 45° C. for 72 hours is 0 to 10% by weight.
[0020] [2] The negative electrode binder composition as described in [1], wherein the hydroxyl group-containing monomer (a) is any one or more selected from the group consisting of 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 3-hydroxypropyl acrylate, 2-hydroxybutyl acrylate, 4-hydroxybutyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, and 4-hydroxybutyl methacrylate.
[0021] [3] The negative electrode binder composition according to [1] or [2], wherein the acid group-containing monomer (b) is neutralized with an alkaline composition or a light metal salt.
[0022] [4] A negative electrode binder composition as described in any one of [1] to [3], wherein the acid group-containing monomer (b) is any one or more selected from the group consisting of acrylic acid, methacrylic acid, maleic acid, monomethyl maleate, 2-carboxyethyl acrylate, 2-carboxyethyl methacrylate, maleic acid, and itaconic acid.
[0023] [5] The negative electrode binder composition as described in any one of [1] to [4], wherein the water-soluble resin (X) further contains one or more selected from the group consisting of acrylamide, methacrylamide, N-methylacrylamide, N,N-dimethylacrylamide, and N-hydroxymethylacrylamide.
[0024] [6] A negative electrode binder composition as described in any one of [1] to [5], wherein the total content of the resin components derived from the aforementioned hydroxyl group-containing monomer (a) and the aforementioned acid group-containing monomer (b) is 5 to 80% by weight relative to the total amount of the aforementioned water-soluble resin (X).
[0025] [7] The negative electrode binder composition as described in any one of [1] to [6], wherein the content of one or more selected from the group consisting of acrylamide, methacrylamide, N-methylacrylamide, N,N-dimethylacrylamide, and N-hydroxymethylacrylamide is 0 to 80% by weight.
[0026] [8] The negative electrode binder composition as described in any one of [1] to [7], wherein the aqueous latex resin (Y) is any one or more of SBR, a styrene acrylate copolymer, and an acrylate copolymer.
[0027] [9] The negative electrode binder composition according to [8], wherein the styrene acrylate copolymer is butyl acrylate.
[0028]
[10] The negative electrode binder composition as described in [9], wherein the content of the constituent units derived from the styrene monomer in the total amount of the styrene acrylate copolymer is 40 to 60% by weight, and the content of the constituent units derived from the butyl acrylate monomer is 20 to 40% by weight.
[0029]
[11] A negative electrode comprising the negative electrode binder composition according to any one of [1] to
[10] as a component.
[0030]
[12] The negative electrode according to
[11] , wherein the total content of the component derived from the water-soluble resin (X) and the component derived from the aqueous latex resin (Y) is 1.5% by weight or more and 5.5% by weight or less.
[0031]
[13] A negative electrode as described in
[11] or
[12] , which contains a graphite-based material as a main active material, and the volume density of the negative electrode is 1.4 g / cm 3 above.
[0032]
[14] The negative electrode according to any one of
[11] to
[13] , wherein the thickness of the mixture layer is 80 μm or more.
[0033]
[15] The negative electrode as described in any one of
[11] to
[14] , which comprises a mixed active material of at least two kinds of materials including a graphite-based material and a silicon-containing material.
[0034]
[16] A secondary battery comprising the negative electrode described in any one of
[11] to
[15] .
[0035]
[17] A method for producing a negative electrode binder composition as described in any one of [1] to
[10] , comprising: a step of thickening an aqueous slurry consisting of at least an active material and the aforementioned water-soluble resin (X); and a subsequent step of reducing the solid content concentration and mixing the aforementioned aqueous latex resin (Y).
[0036] Effects of the Invention
[0037] The negative electrode binder composition of the present invention has good slurry stability even in the absence of a thickener such as cellulose, and has good resistance to electrolyte swelling at high temperatures when it is made into a film. Therefore, the negative electrode containing the negative electrode binder composition of the present invention as a component has strong peel strength, and as a result, when a battery evaluation is performed, even if the number of cycles is high, good charge and discharge characteristics can be exhibited, thereby achieving the performance required for LIB negative electrodes in recent years. DETAILED DESCRIPTION
[0038] <Negative electrode binder composition>
[0039] The negative electrode binder composition of the present invention comprises a water-soluble resin (X) and an aqueous latex resin (Y), wherein the water-soluble resin (X) comprises a copolymer having a hydroxyl group-containing monomer (a) and an acid group-containing monomer (b) as essential components, the weight average molecular weight of the copolymer when measured using an aqueous GPC measuring device is greater than 700,000, and the swelling rate of a dry film of the copolymer after being immersed in a carbonate-based mixed solvent (EC (ethylene carbonate) / DEC (diethylene carbonate) = 50 / 50 (wt)) at 45° C. for 72 hours is 0 to 10% by weight.
[0040] The weight average molecular weight of the copolymer measured using an aqueous GPC measuring device is 700,000 or more, preferably 750,000 to 1,500,000, and more preferably 800,000 to 1,200,000. If the weight average molecular weight is 700,000 or more, as described in the above-mentioned effect of the invention, the slurry stability is good, and the high temperature resistance to electrolyte swelling when the copolymer is made into a film is also good.
[0041] In the above-mentioned aqueous GPC measuring device, a general polymer filler such as polyhydroxymethylacrylate can be used as a column filler. As a column, for example, SB-806HQ, SB-806M HQ of the Shodex OHpak series manufactured by Showa Denko K.K. can be used. In addition, as an eluent, a neutral salt solution such as an aqueous sodium nitrate solution, an aqueous sodium hydrogen hydrochloride solution, an aqueous sodium sulfate solution, and a phosphate buffer solution can be used. As the concentration of these eluents, for example, it is preferably about 0.1 to 0.3 mol / L. As a GPC measuring device, a Shimadzu / L20 system can be used. As a standard substance in the GPC measurement, polystyrene or pullulan can be used. Specifically, as a standard substance, STANDARD P-82 (Pullulan) manufactured by Showa Denko K.K. can be used.
[0042] As described above, the swelling rate of the dried polymer film of the negative electrode binder composition after being immersed in a carbonate-based mixed solvent at 45° C. for 72 hours is 0 to 10% by weight, preferably 0.1 to 6% by weight, and more preferably 0.1 to 4% by weight. The swelling rate is preferably low, and if the swelling rate is within the above range, the peel strength when the negative electrode is made is strong, and as a result, when the battery is evaluated, good charge and discharge characteristics can be exhibited even if the number of cycles is high.
[0043] The above swelling ratio can be obtained as follows: the negative electrode binder composition is dried at room temperature for 72 hours and at 150°C for 30 minutes to prepare a dry polymer film (dried film) with a film thickness of 150 μm, and the dry polymer film is immersed in a carbonate-based mixed solvent (e.g., EC (ethylene carbonate) / DEC (diethylene carbonate) = 50 / 50 (wt.r)) at 60°C for 72 hours, and the weight of the film after immersion is measured, and the weight change rate before and after immersion is set. A high swelling ratio means that the negative electrode binder composition is easy to contain a solvent, and when the negative electrode is made, the substrate such as copper and the mixture are easy to peel (peel).
[0044] [Water-soluble resin (X)]
[0045] As the hydroxyl-containing monomer (a) in the above-mentioned copolymer, for example, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 3-hydroxypropyl acrylate, 2-hydroxybutyl acrylate, 4-hydroxybutyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, and 4-hydroxybutyl methacrylate can be cited. Among them, as the hydroxyl-containing monomer (a), hydroxyethyl acrylate (especially 2-hydroxyethyl acrylate) is preferred. The content of the hydroxyl-containing monomer (a) is, for example, 20 to 80% by weight, preferably 30 to 70% by weight, relative to the total amount of monomers constituting the copolymer. If the content of the hydroxyl-containing monomer (a) is within the above range, there is a tendency that the slurry stability and the resistance to electrolyte swelling at high temperature when the film is made are both good.
[0046] As the acid group-containing monomer (b) in the above-mentioned copolymer, for example, acrylic acid, methacrylic acid, maleic acid, monomethyl maleate, 2-carboxyethyl acrylate, 2-carboxyethyl methacrylate, maleic acid, itaconic acid can be cited. As the acid group in the acid group-containing monomer (b), carboxylic acid is preferred. Among them, as the acid group-containing monomer (b), acrylic acid is particularly preferred. The content of the acid group-containing monomer (b) is, for example, 10 to 60% by weight, preferably 20 to 50% by weight, relative to the total amount of monomers constituting the copolymer. If the content of the acid group-containing monomer (b) is within the above range, there is a tendency that the slurry stability and the resistance to electrolyte swelling at high temperature when the film is made are both good.
[0047] In addition, the acid group-containing monomer (b) in the above copolymer is preferably a substance neutralized with an alkaline composition or a light metal salt. The content of the substance neutralized with an alkaline composition or a light metal salt is, for example, 10 to 60% by weight, preferably 20 to 50% by weight. If these contents are within the above ranges, there is a tendency that the slurry stability and the resistance to electrolyte swelling at high temperatures when the film is made are both good.
[0048] The total content of the resin components derived from the hydroxyl group-containing monomer (a) and the acid group-containing monomer (b) is preferably 5 to 80% by weight, more preferably 10 to 70% by weight, relative to the total amount of the water-soluble resin (X). If the total content is within the above range, the slurry stability and the resistance to electrolyte swelling at high temperature when the film is formed tend to be good.
[0049] The copolymer constituting the water-soluble resin (X) may also contain monomers other than the hydroxyl-containing monomer (a) and the acid-containing monomer (b) (hereinafter referred to as "other monomers (c)"). As other monomers (c), for example, acrylamide, methacrylamide, N-methylacrylamide, N,N-dimethylacrylamide, and N-hydroxymethylacrylamide can be cited. As other monomers (c), acrylamide is preferred, and by including acrylamide, the toughness when the film is made is increased. When other monomers (c) are included, the content of other monomers (c) is, for example, 5 to 40% by weight, preferably 5 to 20% by weight. If the content of other monomers (c) is within the above range, there is a tendency for the resistance to electrolyte swelling at high temperatures to become good.
[0050] The content of any one or more selected from the group consisting of acrylamide, methacrylamide, N-methylacrylamide, N,N-dimethylacrylamide, and N-hydroxymethylacrylamide is 0 to 80% by weight, preferably 2 to 60% by weight. If the content of these is within the above range, there is a tendency that the resistance to electrolyte swelling at high temperature becomes good.
[0051] The copolymer in the water-soluble resin (X) has constituent units derived from the above-mentioned hydroxyl-containing monomer (a) and acid group-containing monomer (b), and other monomers (c) added as needed. The copolymer can be obtained by appropriately adding hydroxyl-containing monomer (a) and acid group-containing monomer (b), and other monomers (c) added as needed, and copolymerizing them using a known and conventional method as described later.
[0052] [Water-based latex resin (Y)]
[0053] Next, as the water-based latex resin (Y), it is preferred to include any one or more of styrene-butadiene copolymer (SBR), styrene acrylate copolymer, and acrylate copolymer. As the water-based latex resin (Y), styrene acrylate copolymer is more preferred. As these acrylates used in the styrene acrylate copolymer, for example, methyl acrylate, methyl methacrylate, butyl acrylate, 2-ethylhexyl acrylate, acrylamide, acrylonitrile, glycidyl methacrylate, etc. can be listed, and acrylic acid, methacrylic acid, etc. can also be used as needed. As the acrylate used in the styrene acrylate copolymer, butyl acrylate is preferred.
[0054] The proportion of the aqueous latex resin (Y) is preferably 20 to 80% by weight, more preferably 30 to 70% by weight, relative to the entire negative electrode binder composition. The content of styrene contained in the styrene acrylate copolymer is 45 to 65% by weight, more preferably 50 to 60% by weight. In addition, the amount of butyl acrylate is preferably 20 to 40% by weight, more preferably 25 to 35% by weight. If the content of styrene and butyl acrylate is within the above range, there is a tendency for the adhesion to become good.
[0055] [Other adhesive ingredients]
[0056] In the negative electrode adhesive composition of the present invention, as an adhesive (binding agent) component, in addition to the above, the components used in the past (referred to as "other adhesive components") may also be included within the scope that does not damage the effect of the present invention. As other adhesive components, there can be listed: (meth) acrylic acid copolymers composed of ethylenically unsaturated carboxylic acid esters (such as methyl (meth) acrylate, ethyl (meth) acrylate, butyl (meth) acrylate, (meth) acrylonitrile, and hydroxyethyl (meth) acrylate, etc.), and ethylenically unsaturated carboxylic acids (such as acrylic acid, methacrylic acid, itaconic acid, fumaric acid, maleic acid, etc.); polymer compounds such as polyvinylidene fluoride, polyethylene oxide, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polyimide, polyamide-imide, and carboxymethyl cellulose (CMC). The negative electrode adhesive composition of the present invention may also contain organic solvents such as N-methyl-2-pyrrolidone (NMP) to dissolve the above polymer compounds.
[0057] The negative electrode mixture slurry and the negative electrode of the present invention include the above-mentioned negative electrode binder composition, and components required for constituting the negative electrode, such as SiO negative electrode material, graphite, acetylene black, etc. In the negative electrode mixture slurry and the negative electrode of the present invention, any type of SiO negative electrode material, graphite, etc. can be used. The proportion (non-volatile component) of the negative electrode binder composition in the negative electrode mixture slurry and the negative electrode of the present invention is, for example, 2 to 10% by weight, preferably 3 to 5% by weight.
[0058] The above-mentioned SiO negative electrode material is a material containing SiO (silicon monoxide) as the main component showing charge and discharge characteristics in the negative electrode of the present invention. In addition to the SiO negative electrode material, silicon particles, carbon, etc. that also show charge and discharge characteristics may also be included. In addition, silicon oxycarbide (SiOC) may also be included as a SiO negative electrode material. These components are not present alone, but may be present in multiple forms. The proportion of the SiO negative electrode material in the negative electrode mixture slurry and the negative electrode of the present invention is, for example, 3 to 20% by weight, preferably 5 to 15% by weight.
[0059] The above-mentioned graphite may be natural graphite or artificial graphite synthesized. Examples of graphite include carbon materials such as natural graphite, artificial graphite, hard carbon, and soft carbon. Graphite is a component that exhibits charge and discharge characteristics, just like SiO negative electrode materials. The proportion of graphite in the negative electrode mixture slurry and the negative electrode of the present invention is, for example, 80 to 97% by weight, preferably 85 to 95% by weight.
[0060] The acetylene black acts as a conductive aid in the negative electrode of the present invention, and may also be carbon black, Ketjen black, carbon nanotubes (CNTs) and the like, which are components other than acetylene black. The proportion of these components acting as conductive aids in the negative electrode mixture slurry and the negative electrode of the present invention is, for example, 0.05 to 10% by weight, preferably 0.1 to 5% by weight.
[0061] The solvent used in the negative electrode mixture slurry of the present invention is not particularly limited, as long as it can disperse the components required to constitute the negative electrode mixture slurry. An aqueous solvent can be used, preferably ion-exchanged water. The proportion of the solvent in the negative electrode mixture slurry is, for example, 30 to 70% by weight, preferably 40 to 60% by weight.
[0062] [Method for producing negative electrode binder composition]
[0063] An example of a method for producing the negative electrode binder composition of the present invention is described below. The method for producing the negative electrode binder composition of the present invention preferably comprises: a step of thickening an aqueous slurry composed of at least an active material and a water-soluble resin (X); and a step of subsequently reducing the solid content concentration and mixing an aqueous latex resin (Y).
[0064] First, a copolymer of a water-soluble resin (X) which is an essential component of the negative electrode binder composition is synthesized. The copolymer can be obtained by adding a solvent such as water to a reaction vessel and heating it to 50-80°C, then adding a hydroxyl-containing monomer (a) and an acid-containing monomer (b), other monomers (c) as optional components, and a mixture of polymerization initiators such as ammonium persulfate to carry out a polymerization reaction. The polymerization reaction can also be carried out in an inert gas environment such as nitrogen. The polymerization reaction can be carried out at a temperature of 50-80°C for 1-10 hours. After the reaction is completed, it is cooled and the pH is adjusted.
[0065] Then, active material, other adhesive components, water, and organic solvent are added to the obtained water-soluble resin (X) containing copolymers, and the water-based slurry composed of these components is thickened. The active material can be any one of tin alloy, silicon alloy, silicon oxide, etc. As other adhesive components, for example, high molecular weight compounds such as ethylenically unsaturated carboxylic acids and ethylenically unsaturated carboxylic acid esters can be listed. As an organic solvent, N-methyl-2-pyrrolidone (NMP) is preferred. The thickening can be carried out by putting in a specified amount at one time, or after putting in about half of the specified amount of each component and thickening once, the total amount of the specified amount is put in and thickened twice. The process of defoaming the water-based slurry can also be appropriately increased.
[0066] Next, after the aqueous slurry is thickened, the solid content concentration of the slurry is reduced and an aqueous latex resin (Y) is mixed to obtain a negative electrode binder composition. The amount of the aqueous latex resin (Y) is, for example, 50 to 300 parts by weight, preferably 80 to 200 parts by weight, relative to 100 parts by weight of the water-soluble resin (X).
[0067] Furthermore, the negative electrode mixture slurry is obtained by adding SiO negative electrode material, graphite, acetylene black, solvent and other components required for the negative electrode to the above-mentioned negative electrode binder composition, and dispersing them in an aqueous solvent such as ion exchange water. Dispersion can be performed using a dispersing device such as a stirrer, a ball mill, a super sand mill, a pressure kneader, etc. In addition, the negative electrode mixture slurry can also be prepared by mixing using a mixer.
[0068] <Negative electrode>
[0069] The negative electrode of the present invention comprises the above-mentioned negative electrode binder composition as a component. In the negative electrode of the present invention, the total content of the component derived from the water-soluble resin (X) and the component derived from the water-based latex resin (Y) is preferably 1.5 wt% or more and 5.5 wt% or less, and more preferably 2.0 wt% or more and 5.0 wt% or less. In addition, the negative electrode of the present invention preferably comprises a graphite-based material as the main active material, and the volume density of the negative electrode is 1.4 g / cm 3 In addition, a mixed active material of at least two materials including a graphite-based material and a silicon-containing material is preferred. Furthermore, the negative electrode of the present invention preferably has a mixture layer with a thickness of 80 μm or more.
[0070] The negative electrode of the present invention can be obtained by coating the negative electrode mixture slurry containing the negative electrode binder composition obtained above on the collector copper foil to form a negative electrode layer as a thin film. In addition, the negative electrode mixture slurry as the negative electrode binder composition can also be formed into a sheet, granular or other shape as described later, and integrated with the collector to obtain the negative electrode.
[0071] The material and shape of the current collector are not particularly limited, and may be made of, for example, copper, nickel, titanium, stainless steel, etc., in the form of a foil, perforated foil, mesh, etc. Alternatively, porous materials, such as porous metal (foamed metal), carbon paper, etc. may be used.
[0072] The method for coating the copper foil of the current collector is not particularly limited, and examples thereof include metal shield printing, electrostatic coating, dip coating, spray coating, roll coating, blade coating, gravure coating, screen printing, and other known methods. After coating, it is preferably rolled by a flat press, a roller, or the like as needed.
[0073] In addition, the negative electrode mixture slurry formed into a sheet, granule or other shape and the current collector can be integrated by a known method such as a roller, a press, or a combination of these. The electrode density after integration is, for example, 1.0 to 1.8 g / cm 3 , preferably 1.1 to 1.7 g / cm 3 .
[0074] The negative electrode layer formed on the above-mentioned current collector and the negative electrode layer integrated with the current collector are preferably heat-treated. The heat treatment conditions are, for example, 80 to 150° C. and 5 to 20 hours. The solvent is removed by the heat treatment, and the binder is hardened, thereby performing high strength, thereby improving the adhesion between particles and between particles and the current collector. Furthermore, in order to prevent oxidation of the current collector during the treatment process, these heat treatments are preferably performed in an inactive environment such as helium, argon, nitrogen, or a vacuum environment.
[0075] <Secondary battery>
[0076] The secondary battery of the present invention is composed of the negative electrode of the present invention. When used as a wet electrolyte secondary battery, for example, the secondary battery of the present invention can be constructed by arranging a positive electrode and a negative electrode of the present invention facing each other via a separator and injecting an electrolyte.
[0077] The positive electrode can be obtained by forming a positive electrode layer on the surface of a current collector, similarly to the negative electrode. The current collector in this case can be made of a metal such as aluminum, titanium, stainless steel, or an alloy in the form of a foil, perforated foil, mesh, or other strip.
[0078] There is no particular restriction on the positive electrode material used for the positive electrode layer. In the case of a secondary battery, when a lithium-ion secondary battery is manufactured, for example, a metal compound, metal oxide, metal sulfide, or conductive polymer material that can be doped or inserted with lithium ions can be used without particular restriction. For example, lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganese oxide (LiMnO 2), and their composite oxides (LiCo x Ni y Mn z O 2 , x+y+z=1), lithium manganese spinel (LiMn 2 O 4 ), lithium vanadium compounds, V 2 O 5 、V 6 O 13 , VO 2 、MnO 2 、TiO 2 、MoV 2 O 8 、TiS 2 、V 2 S 5 VS 2 、MoS 2 、MoS 3 Cr 3 O 8 Cr 2 O 5 , Olivine LiMPO 4 (M: Co, Ni, Mn, Fe), conductive polymers such as polyacetylene, polyaniline, polypyrrole, polythiophene, polyacene, porous carbon, etc. can be used alone or in combination.
[0079] As the separator, for example, a nonwoven fabric, a cloth, a microporous membrane or a separator formed by combining polyolefins such as polyethylene and polypropylene as the main component can be used. Furthermore, in the case of a structure in which the positive electrode and the negative electrode of the nonaqueous electrolyte secondary battery to be manufactured do not directly contact each other, it is not necessary to use a separator.
[0080] As the electrolyte, for example, LiClO 4 、LiPF 6 、LiAsF 6 , LiBF 4 、LiSO 3 CF 3 The so-called organic electrolyte solution is formed by dissolving lithium salts such as ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, fluoroethylene carbonate, cyclopentanone, sulfolane, 3-methylsulfolane, 2,4-dimethylsulfolane, 3-methyl-1,3-oxazolidin-2-one, γ-butyrolactone, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, methyl butyl carbonate, ethyl propyl carbonate, ethyl butyl carbonate, dipropyl carbonate, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, methyl acetate, ethyl acetate and the like in a single body or a mixture of two or more components in a non-aqueous solvent.
[0081] The structure of the secondary battery of the present invention is not particularly limited. Generally, the positive electrode, the negative electrode, and the separator provided as required are usually wound into a flat spiral to form a spiral electrode plate group, or these are stacked in a flat plate shape to form a stacked electrode plate group, and these electrode plate groups are sealed in an outer body.
[0082] The secondary battery of the present invention is not particularly limited and can be used in the form of a paper battery, a button battery, a coin battery, a laminated battery, a cylindrical battery, a square battery, etc. The negative electrode active material of the present invention can also be applied to all electrochemical devices that use lithium ion insertion and removal as a charging and discharging mechanism, such as hybrid capacitors, solid lithium secondary batteries, etc.
[0083] Example
[0084] Hereinafter, the present invention will be described in detail by way of examples.
[0085] Synthesis Example 1, Synthesis Example 4, and Synthesis Example 5 are methods for synthesizing a water-soluble resin (X) containing a copolymer containing a hydroxyl group-containing monomer (a) and an acid group-containing monomer (b) as essential components. In addition, Synthesis Examples 6 to 15 are methods for synthesizing a water-soluble resin (X) further containing another monomer (c). Synthesis Example 2 is a method for synthesizing a water-soluble resin (X) having a molecular weight of 700,000 or less as a water-soluble resin (X) used in a comparative example. Synthesis Example 16 is a method for synthesizing a water-soluble resin (X) obtained by removing an acid group-containing monomer (b) from the water-soluble resin (X) of the present invention. Synthesis Example 17 is a method for synthesizing a water-soluble resin (X) obtained by removing a hydroxyl group-containing monomer (a) from the water-soluble resin (X) of the present invention. In addition, Synthesis Examples 18 to 20 are methods for synthesizing an aqueous latex resin (Y) composed of a styrene acrylate copolymer, and Synthesis Example 21 is a method for synthesizing an aqueous latex resin (Y) composed of an acrylate copolymer.
[0086] Negative electrode mixture slurry preparation example 1 is an example of using the water-soluble resin (X) of the present invention containing a copolymer containing a hydroxyl group-containing monomer (a) and an acid group-containing monomer (b) as essential components (Synthesis Example 1) and using SBR as the aqueous latex (Y), and negative electrode mixture slurry preparation examples 2 to 4 are examples of using the water-soluble resin (X) of the present invention containing a copolymer containing a hydroxyl group-containing monomer (a) and an acid group-containing monomer (b) as essential components (Synthesis Example 1, Synthesis Example 4, Synthesis Example 5) and using a styrene acrylate copolymer (Synthesis Example 18) as the aqueous latex (Y). In addition, negative electrode mixture slurry preparation examples 5 to 13 are examples of the water-soluble resin (X) of the present invention further containing other monomers (c) (Synthesis Examples 7 to 8, Synthesis Examples 11 to 15) and using a styrene acrylate copolymer (Synthesis Examples 18 to 20) as the aqueous latex (Y). Negative electrode mixture slurry preparation example 14 is an example in which the water-soluble resin (X) of the present invention further contains other monomers (c) (Synthesis Example 8) and the aqueous latex (Y) uses an acrylate copolymer (Synthesis Example 21). Negative electrode mixture slurry preparation examples 15-16 are examples in which the water-soluble resin (X) of the present invention further contains other monomers (c), the acid group-containing monomer (b) is a substance neutralized with a light metal hydroxide (Synthesis Example 9 (Li salt), Synthesis Example 10 (Na salt)), and the aqueous latex (Y) uses a styrene acrylate copolymer (Synthesis Example 18). Negative electrode mixture slurry preparation examples 17-18 are examples in which the water-soluble resin (X) of the present invention further contains other monomers (c) (Synthesis Example 8) and the aqueous latex (Y) uses a styrene acrylate copolymer (Synthesis Example 18), and the amount of binder added is further increased or decreased. In addition, negative electrode mixture slurry preparation examples 19 to 20 are examples in which the water-soluble resin (X) of the present invention further contains other monomers (c) (Synthesis Example 8) and the aqueous latex (Y) uses a styrene acrylate copolymer (Synthesis Example 18), and the active material uses a mixture of a graphite-based material and a material containing silicon.
[0087] Negative electrode mixture slurry preparation example 21 is an example of using CMC and SBR. In addition, negative electrode mixture slurry preparation example 22 is an example of using only a water-soluble resin (X) (Synthesis Example 1) containing a copolymer containing a hydroxyl-containing monomer (a) and an acid-containing monomer (b) as essential components. Negative electrode mixture slurry preparation example 23 is an example of using CMC and using a styrene acrylate copolymer as the aqueous latex resin (Y) (Synthesis Example 18). Negative electrode mixture slurry preparation example 24 is an example of using a water-soluble resin (X) (Synthesis Example 2) containing a copolymer containing a hydroxyl-containing monomer (a) and an acid-containing monomer (b) as essential components and having a molecular weight of less than 700,000 and using a styrene acrylate copolymer as the aqueous latex (Y) (Synthesis Example 18). Negative electrode mixture slurry preparation example 25 is an example of using a water-soluble resin (X) that makes the swelling rate of the dried polymer film 10% or more after immersion in a carbonate-based mixed solvent at 45°C for 72 hours, and using a styrene acrylate copolymer (Synthesis Example 18) as the aqueous latex (Y). Negative electrode mixture slurry preparation example 26 is an example of using an unneutralized water-soluble resin (X) (Synthesis Example 6) containing a copolymer containing a hydroxyl-containing monomer (a) and an acid-containing monomer (b) as essential components, and using a styrene acrylate copolymer (Synthesis Example 18) as the aqueous latex (Y). Slurry preparation example 27 is an example of using a water-soluble resin (X) (Synthesis Example 16) obtained by removing the acid-containing monomer (b) from the water-soluble resin (X) of the present invention, and using a styrene acrylate copolymer (Synthesis Example 18) as the aqueous latex (Y). Slurry Preparation Example 28 is an example of using a water-soluble resin (X) (Synthesis Example 17) obtained by removing a hydroxyl-containing monomer (a) from the water-soluble resin (X) of the present invention, and using a styrene acrylate copolymer (Synthesis Example 18) as the aqueous latex (Y). Slurry Preparation Example 29 is an example of using commercially available sodium polyacrylate and using a styrene acrylate copolymer (Synthesis Example 18) as the aqueous latex (Y). In addition, negative electrode mixture slurry preparation examples 30 to 31 are examples of using CMC and SBR and increasing or decreasing the amount of binder added. In addition, negative electrode mixture slurry preparation examples 32 to 33 are examples of using CMC and SBR and using a mixture of a graphite-based material and a silicon-containing material as the active material.
[0088] As the water-soluble resin (X) used in the comparative example, CMC (sodium salt of carboxymethylcellulose, SUNROSE MAC350 manufactured by Nippon Paper Industries) and PAA-Na (sodium polyacrylate, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., with a polymerization degree of 22,000 to 70,000) were used. In addition, as the water-based latex resin (Y) used in the examples and comparative examples, SBR (styrene butadiene copolymer, LUXSTAR DS407H manufactured by DIC Corporation) was used.
[0089] Positive Electrode Preparation Examples 1 to 3 show the preparation methods of the positive electrodes used in the batteries of the Examples and Comparative Examples. Next, the preparation methods of the negative electrodes of the present invention are shown in Examples 1 to 24, and the preparation methods of the batteries of the present invention are shown in Examples 25 to 48. In addition, the preparation methods of the negative electrodes of the Comparative Examples are shown in Comparative Examples 1 to 17, and the preparation methods of the batteries of the Comparative Examples are shown in Comparative Examples 18 to 34.
[0090] [Aqueous GPC measurement]
[0091] In the aqueous GPC measurement, the Shimadzu / L20 system was used as the HPLC apparatus, and the column was Shodex OHpakSB-806MHQ (8.0 mmI.D.×300 mmL.×2). The eluent was a 0.2 mol / L sodium nitrate aqueous solution, and the sample was dissolved in a manner of 0.5%, and the measurement was performed after filtering with a φ0.45 filter. 50 μL of the sample was added, and the weight average molecular weight was determined using an RI detector while flowing at a flow rate of 0.70 mL / min. The standard substance was STANDARD P-82 (Pullulan) manufactured by Showa Denko, and a calibration curve was prepared.
[0092] "Synthesis example of a water-soluble resin (X) comprising a copolymer containing a hydroxyl group-containing monomer (a) and an acid group-containing monomer (b) as essential components"
[0093] [Synthesis example 1]
[0094] In a 1.0 L reaction vessel equipped with a stirrer, a thermometer, a cooler, and a nitrogen blowing device, 500.0 parts by weight of ion exchange water was added and nitrogen blowing was performed for 3 hours. 2 Then heat to 75°C. A mixture of 40.0 parts by weight of acrylic acid, 60.0 parts by weight of hydroxyethyl acrylate, 0.367 parts by weight of ammonium persulfate (1500 ppm relative to the total molar number of monomers), and 50.0 parts by weight of ion exchange water was added dropwise over 3 hours to carry out a polymerization reaction. After the addition is completed, keep at the same temperature for 2 hours and then cool. Add 5 mol / L sodium hydroxide aqueous solution and distilled water at a temperature below 40°C, adjust the pH to the range of 6.8 to 7.2, and adjust the non-volatile component to the range of 14.8% by weight to 15.2% by weight. The copolymer thus obtained has a non-volatile component of 14.8% by weight, a pH of 6.8, a viscosity of 3080 mPa·s, and a weight average molecular weight of 850,000 measured by aqueous GPC.
[0095] (Measurement of Swelling Degree in Carbonate Mixed Solvent)
[0096] After the obtained copolymer solution is coated on a PET film, it is left to dry at room temperature for 3 days to form a copolymer film. After peeling it off, it is cut into 1.0 cm × 1.0 cm squares, then dried in an air drier at 80°C for 1 hour, and then dried in a vacuum drier at 110°C for 10 hours. The thickness of the obtained film is 100 to 150 μm. After measuring the weight of the film, it is immersed in a carbonate mixed solvent (EC (ethylene carbonate) / DEC (diethylene carbonate) = 50 / 50 (wt)) at 45°C for 72 hours, and the weight of the film is measured again. The swelling degree for the carbonate mixed solvent calculated according to the following formula (1) is 5.3%.
[0097] {(weight of film after immersion - weight of film before immersion) / (weight of film before immersion)}×100 Formula (1)
[0098] [Synthesis example 2]
[0099] Except for the case where 3 hours of blowing is not carried out 2 The polymerization reaction was carried out in the same manner as in Synthesis Example 1 except for the above. The nonvolatile content of the copolymer thus obtained was 15.0% by weight, the pH was 6.8, the viscosity was 1380 mPa·s, and the weight average molecular weight measured by aqueous GPC was 480,000. In addition, the swelling degree in the carbonate mixed solvent was 5.3%.
[0100] [Synthesis example 3]
[0101] The polymerization reaction was carried out in the same manner as in Synthesis Example 1 except that 20.0 parts by weight of acrylic acid, 80.0 parts by weight of hydroxyethyl acrylate and 0.340 parts by weight of ammonium persulfate (1500 ppm relative to the total molar number of monomers) were used. The nonvolatile component of the copolymer thus obtained was 14.9% by weight, the pH was 7.0, the viscosity was 2800 mPa·s, and the weight average molecular weight measured by water-based GPC was 750,000. In addition, the swelling degree for the carbonate mixed solvent was 26.9%.
[0102] [Synthesis Example 4]
[0103] The polymerization reaction was carried out in the same manner as in Synthesis Example 1 except that 60.0 parts by weight of 4-hydroxybutyl acrylate and 0.332 parts by weight of ammonium persulfate (1500 ppm relative to the total molar number of the monomers) were used instead of 60.0 parts by weight of hydroxyethyl acrylate. The nonvolatile content of the copolymer thus obtained was 15.1% by weight, the pH was 6.9, the viscosity was 3000 mPa·s, and the weight average molecular weight measured by aqueous GPC was 800,000. In addition, the swelling degree for the carbonate mixed solvent was 6.2%.
[0104] [Synthesis Example 5]
[0105] The polymerization reaction was carried out in the same manner as in Synthesis Example 1 except that 40.0 parts by weight of 2-carboxyethyl acrylate and 0.272 parts by weight of ammonium persulfate (1500 ppm relative to the total molar number of the monomers) were used instead of 40.0 parts by weight of acrylic acid. The nonvolatile component of the copolymer thus obtained was 14.9% by weight, the pH was 6.9, the viscosity was 3000 mPa·s, and the weight average molecular weight measured by water-based GPC was 840,000. In addition, the swelling degree for the carbonate mixed solvent was 5.5%.
[0106] [Synthesis example 6]
[0107] The reaction was carried out in the same manner as in Synthesis Example 1 except that a 5 mol / L sodium hydroxide aqueous solution was not added to adjust the pH. The nonvolatile content was 15.0% by weight, the pH was 3.8, the viscosity was 2050 mPa·s, and the weight average molecular weight measured by aqueous GPC was 830,000. In addition, the degree of swelling in the carbonate mixed solvent was 5.8%.
[0108] [Synthesis Example 7]
[0109] In a 1.0 L reaction vessel equipped with a stirrer, a thermometer, a cooler, and a nitrogen blowing device, 500.0 parts by weight of ion exchange water was added and nitrogen blowing was performed for 3 hours. 2 Then heat to 75°C. A mixture of 30.0 parts by weight of acrylic acid, 60.0 parts by weight of hydroxyethyl acrylate, 10.0 parts by weight of acrylamide, 0.443 parts by weight of ammonium persulfate (1500ppm relative to the total molar number of monomers), and 50.0 parts by weight of ion exchange water was added dropwise over a period of 3 hours to carry out a polymerization reaction. After the addition was completed, it was kept at the same temperature for 2 hours and then cooled. 5 mol / L sodium hydroxide aqueous solution and distilled water were added at a temperature below 40°C, the pH was adjusted to a range of 6.8 to 7.2, and the non-volatile component was adjusted to a range of 14.8% by weight to 15.2% by weight. The non-volatile component of the obtained copolymer was 15.0% by weight, the pH was 7.1, the viscosity was 3100mPa·s, and the weight average molecular weight measured by aqueous GPC was 730,000. In addition, the degree of swelling for a carbonate mixed solvent was 4.2%.
[0110] [Synthesis example 8]
[0111] The polymerization reaction was carried out in the same manner as in Synthesis Example 7 except that 20.0 parts by weight of acrylic acid, 20.0 parts by weight of hydroxyethyl acrylate, 60.0 parts by weight of acrylamide, 0.405 parts by weight of ammonium persulfate (1500 ppm relative to the total molar number of monomers) and 25% ammonia water were used instead of 5 mol / L sodium hydroxide aqueous solution. The nonvolatile component of the obtained copolymer was 15.0% by weight, pH was 7.0, viscosity was 12500 mPa·s, and weight average molecular weight measured by water-based GPC was 780,000. In addition, the swelling degree for carbonate mixed solvent was 4.5%.
[0112] [Synthesis Example 9]
[0113] The polymerization reaction was carried out in the same manner as in Synthesis Example 7 except that 20.0 parts by weight of acrylic acid, 20.0 parts by weight of hydroxyethyl acrylate, 60.0 parts by weight of acrylamide, and 0.405 parts by weight of ammonium persulfate (1500 ppm relative to the total molar number of monomers) were used. The nonvolatile component of the obtained copolymer was 15.0% by weight, the pH was 7.0, the viscosity was 13700 mPa·s, and the weight average molecular weight measured by water-based GPC was 780,000. In addition, the swelling degree for the carbonate mixed solvent was 6.0%.
[0114] [Synthesis Example 10]
[0115] The polymerization reaction was carried out in the same manner as in Synthesis Example 7 except that 20.0 parts by weight of acrylic acid, 20.0 parts by weight of hydroxyethyl acrylate, 60.0 parts by weight of acrylamide, 0.405 parts by weight of ammonium persulfate (1500 ppm relative to the total molar number of monomers) and 5 mol / L lithium hydroxide aqueous solution were used instead of 5 mol / L sodium hydroxide aqueous solution. The nonvolatile component of the obtained copolymer was 15.0% by weight, pH was 7.0, viscosity was 13200 mPa·s, and weight average molecular weight measured by water-based GPC was 780,000. In addition, the swelling degree for carbonate mixed solvent was 5.3%.
[0116] [Synthesis Example 11]
[0117] The polymerization reaction was carried out in the same manner as in Synthesis Example 7 except that 20.0 parts by weight of acrylic acid, 20.0 parts by weight of hydroxyethyl acrylate, 60.0 parts by weight of hydroxymethyl acrylamide was used instead of acrylamide, 0.357 parts by weight of ammonium persulfate (1500 ppm relative to the total molar number of monomers), and 25% ammonia water was used instead of 5 mol / L sodium hydroxide aqueous solution. The nonvolatile component of the obtained copolymer was 15.0% by weight, pH was 7.0, viscosity was 17100 mPa·s, and weight average molecular weight measured by aqueous GPC was 830,000. In addition, the swelling degree for carbonate mixed solvent was 4.6%.
[0118] [Synthesis Example 12]
[0119] The polymerization reaction was carried out in the same manner as in Synthesis Example 7 except that 10.0 parts by weight of acrylic acid, 10.0 parts by weight of hydroxyethyl acrylate, 80.0 parts by weight of acrylamide, 0.438 parts by weight of ammonium persulfate (1500 ppm relative to the total molar number of monomers) and 25% ammonia water were used instead of 5 mol / L sodium hydroxide aqueous solution. The nonvolatile component of the obtained copolymer was 14.9% by weight, the pH was 7.0, the viscosity was 15200 mPa·s, and the weight average molecular weight measured by water-based GPC was 860,000. In addition, the swelling degree for the carbonate mixed solvent was 6.2%.
[0120] [Synthesis Example 13]
[0121] The polymerization reaction was carried out in the same manner as in Synthesis Example 7 except that 35.0 parts by weight of acrylic acid, 35.0 parts by weight of hydroxyethyl acrylate, 30.0 parts by weight of acrylamide, 0.414 parts by weight of ammonium persulfate (1500 ppm relative to the total molar number of monomers) and 25% ammonia water were used instead of 5 mol / L sodium hydroxide aqueous solution. The nonvolatile component of the obtained copolymer was 15.0% by weight, the pH was 7.0, the viscosity was 13300 mPa·s, and the weight average molecular weight measured by water-based GPC was 840,000. In addition, the swelling degree for the carbonate mixed solvent was 6.0%.
[0122] [Synthesis Example 14]
[0123] The polymerization reaction was carried out in the same manner as in Synthesis Example 7 except that 20.0 parts by weight of acrylic acid, 40.0 parts by weight of hydroxyethyl acrylate, 40.0 parts by weight of acrylamide, 0.442 parts by weight of ammonium persulfate (1500ppm relative to the total molar number of monomers) and 25% ammonia water were used instead of 5 mol / L sodium hydroxide aqueous solution. After the addition was completed, the mixture was kept at the same temperature for 2 hours and then cooled. Ammonia solution was added at a temperature below 40°C for pH adjustment. The nonvolatile component of the copolymer obtained was 15.1% by weight, the pH was 7.0, the viscosity was 14500mPa·s, and the weight-average molecular weight measured by aqueous GPC was 830,000. In addition, the degree of swelling in a carbonate mixed solvent was 5.8%.
[0124] [Synthesis Example 15]
[0125] The polymerization reaction was carried out in the same manner as in Synthesis Example 7 except that 30.0 parts by weight of acrylic acid, 20.0 parts by weight of hydroxyethyl acrylate, 50.0 parts by weight of acrylamide, 0.424 parts by weight of ammonium persulfate (1500ppm relative to the total molar number of monomers) and 25% ammonia water were used instead of 5 mol / L sodium hydroxide aqueous solution. After the addition was completed, the mixture was kept at the same temperature for 2 hours and then cooled. Ammonia solution was added at a temperature below 40°C for pH adjustment. The nonvolatile component of the copolymer obtained was 15.1% by weight, the pH was 7.0, the viscosity was 13000mPa·s, and the weight-average molecular weight measured by aqueous GPC was 840,000. In addition, the degree of swelling in a carbonate mixed solvent was 5.3%.
[0126] [Synthesis Example 16]
[0127] In a 1.0 L reaction vessel equipped with a stirrer, a thermometer, a cooler, and a nitrogen blowing device, 500.0 parts by weight of ion exchange water was added and nitrogen blowing was performed for 3 hours. 2 Then heat to 75°C. A mixture of 70.0 parts by weight of hydroxyethyl acrylate, 30.0 parts by weight of acrylamide, 0.351 parts by weight of ammonium persulfate (1500 ppm relative to the total molar number of monomers), and 50.0 parts by weight of ion exchange water was added dropwise over 3 hours to carry out polymerization reaction. After the addition was completed, the mixture was kept at the same temperature for 2 hours and then cooled. The nonvolatile component of the obtained copolymer was 15.0% by weight, the pH was 7.0, the viscosity was 4300 mPa·s, and the weight average molecular weight measured by aqueous GPC was 750,000. In addition, the swelling degree for carbonate mixed solvent was 17.5%.
[0128] [Synthesis Example 17]
[0129] In a 1.0 L reaction vessel equipped with a stirrer, a thermometer, a cooler, and a nitrogen blowing device, 500.0 parts by weight of ion exchange water was added and nitrogen blowing was performed for 3 hours. 2Then heat to 75°C. A mixture of 70.0 parts by weight of hydroxyethyl acrylate, 30.0 parts by weight of acrylamide, 0.351 parts by weight of ammonium persulfate (1500ppm relative to the total molar number of monomers), and 50.0 parts by weight of ion exchange water was added dropwise over a period of 3 hours to carry out a polymerization reaction. After the addition was completed, it was kept at the same temperature for 2 hours and then cooled. 5 mol / L sodium hydroxide aqueous solution and distilled water were added at a temperature below 40°C, the pH was adjusted to a range of 6.8 to 7.2, and the non-volatile component was adjusted to a range of 14.8% by weight to 15.2% by weight. The non-volatile component of the obtained copolymer was 15.0% by weight, the pH was 7.0, the viscosity was 8900mPa·s, and the weight average molecular weight measured by aqueous GPC was 820,000. In addition, the degree of swelling for a carbonate mixed solvent was 5.1%.
[0130] The monomer composition (wt%), the presence or absence of blowing in the "Synthesis Examples of Water-soluble Resin (X) Containing a Copolymer Including a Hydroxyl-containing Monomer (a) and an Acid-containing Monomer (b) as Essential Components" of Synthesis Examples 1 to 17 were compared. 2 , the base used for neutralization, the non-volatile content, pH, viscosity, the weight average molecular weight of the polymer, and the swelling degree for the carbonate mixed solvent are summarized and shown in the following Table 1.
[0131] Synthesis Example of a Water-Soluble Resin (X) Containing a Copolymer Including a Hydroxyl-Containing Monomer (a) and an Acid-Containing Monomer (b) as Essential Components
[0132] [Table 1]
[0133]
[0134] "Synthesis Example of Water-Based Latex Resin (Y)"
[0135] [Synthesis Example 18]
[0136] 450 parts by mass of ion exchange water was added to a 2 L reaction vessel equipped with a stirrer, a thermometer, a cooler, and a nitrogen blowing device, and nitrogen blowing was performed for 3 hours. 2Afterwards, the mixture was heated to 80°C. An emulsion prepared by emulsifying 272.5 parts by weight of styrene, 150 parts by weight of n-butyl acrylate, 40 parts by weight of hydroxyethyl methacrylate, 25 parts by weight of methacrylic acid, 10 parts by weight of acrylamide, 2.5 parts by weight of glycidyl methacrylate, 10 parts by weight of sodium dodecylbenzenesulfonate, 1.25 parts by weight of ammonium persulfate, and 120 parts by weight of ion exchange water was added dropwise over 3 hours to carry out emulsion polymerization. After stirring at 80°C for 2 hours, the mixture was cooled to below 40°C, and the pH was adjusted to 6 to 7 with aqueous ammonia, and the nonvolatile content was adjusted to 39 to 41% with ion exchange water. The nonvolatile content of the obtained water-based latex resin was 39.6%, the viscosity was 28 mPa·s, and the pH was 6.9.
[0137] [Synthesis Example 19]
[0138] The polymerization reaction was carried out in the same manner as in Synthesis Example 14 except that 172.5 parts by weight of styrene and 250 parts by weight of n-butyl acrylate were used. The mixture was cooled to 40° C. or less, the pH was adjusted to 6 to 7 with aqueous ammonia, and the nonvolatile content was adjusted to 39 to 41% with ion exchange water. The nonvolatile content of the obtained polymer emulsion was 40.5%, the viscosity was 31 mPa·s, and the pH was 7.0.
[0139] [Synthesis Example 20]
[0140] The polymerization reaction was carried out in the same manner as in Synthesis Example 14 except that 222.5 parts by weight of styrene and 220 parts by weight of n-butyl acrylate were used. The mixture was cooled to 40° C. or less, the pH was adjusted to 6 to 7 with aqueous ammonia, and the nonvolatile content was adjusted to 39 to 41% with ion exchange water. The nonvolatile content of the obtained polymer emulsion was 40.0%, the viscosity was 27 mPa·s, and the pH was 7.0.
[0141] [Synthesis Example 21]
[0142] The polymerization reaction was carried out in the same manner as in Synthesis Example 14 except that 272.5 parts by weight of benzyl acrylate was used instead of styrene. The mixture was cooled to below 40°C, the pH was adjusted to 6 to 7 with aqueous ammonia, and the nonvolatile content was adjusted to 39 to 41% with ion exchange water. The nonvolatile content of the obtained polymer emulsion was 40.0%, the viscosity was 34 mPa·s, and the pH was 7.0.
[0143] The monomer composition (weight %), base used for neutralization, pH, weight average molecular weight of the polymer, nonvolatile content, and viscosity in the above-mentioned Synthesis Examples 18 to 21 of the "Synthesis Examples of Water-Based Latex Resin (Y)" are summarized and shown in Table 2 below.
[0144] Synthesis Example of Water-Based Latex Resin (Y)
[0145] [Table 2]
[0146] Resin Name Synthesis Example 18 Synthesis example 19 Synthesis example 20 Synthesis Example 21 Hydroxyethyl Methacrylate (HEMA) 8 8 8 8 Acrylamide (AAM) 2 2 2 2 Methacrylic acid (MAA) 5 5 5 5 Styrene (ST) 54.5 34.5 44.5 0 Benzyl acrylate(BNA) 0 0 0 54.5 Butyl acrylate (BA) 30 50 40 30 Glycidyl Methacrylate (GMA) 0.5 0.5 0.5 0.5 Base used for neutralization NH3 NH3 NH3 NH3 Non-volatile components (%) 40.2 40.5 40 40 DH 7 7 7 7 Viscosity (mPa·s) 30 31 27 34
[0147] "Example of preparing negative electrode mixture slurry"
[0148] [Slurry Preparation Example 1]
[0149] 96.0 parts by weight of artificial graphite (initial charge capacity 390 mAh / g, initial discharge capacity 350 mAh / g) and 1.0 parts by weight of acetylene black were weighed and stirred for 30 seconds using a rotation-revolution mixer (ARE-310 manufactured by Thinky Co., Ltd.) at a rotation of 1000 rpm and a revolution of 2000 rpm. 27.0 parts by weight (1.08 parts by weight in terms of solid content conversion weight) of an aqueous solution prepared by diluting the binder composition (HEA / AA=60 / 40, Na salt, weight average molecular weight 850000, non-volatile component concentration 14.8%) shown in Synthesis Example 1 above with distilled water and adjusting the non-volatile component concentration to 4.0% and 25.0 parts by weight of distilled water were added and mixed until the whole became a paste. Next, the mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm in a rotation and revolution mixer (ARE-310 manufactured by Thinky). Heat was released by stirring, so the mixture was cooled to room temperature with ice water. The mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm, and then cooled to room temperature with ice water. 10.5 parts by weight (0.42 parts by weight in terms of non-volatile component conversion) of an aqueous solution of the adhesive composition of Synthesis Example 1 prepared previously to a non-volatile component concentration of 4% was added and mixed until the whole mixture became uniform. The mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm in a rotation and revolution mixer (ARE-310 manufactured by Thinky), and then cooled to room temperature with ice water. Add 7 parts by weight of distilled water and 2.95 parts by weight of styrene butadiene copolymer (SBR) (DS407H manufactured by DIC, non-volatile component concentration 50.8%), and use a rotation / revolution mixer (ARE-310 manufactured by Thinky) to stir for 30 seconds at a rotation of 1000 rpm and a revolution of 2000 rpm to prepare a negative electrode mixture slurry.
[0150] [Slurry Preparation Example 2]
[0151] A negative electrode mixture slurry was prepared in the same manner as in slurry preparation example 1, except that 3.73 parts by weight of the aqueous latex resin (Y) (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile matter concentration 40.2%) synthesized in synthesis example 18 was used instead of SBR.
[0152] [Slurry Preparation Example 3]
[0153] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in synthesis example 4 (HBA / AA=60 / 40, Na salt, weight average molecular weight 800,000, non-volatile component concentration 15.1%) is used instead of synthesis example 1, and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in synthesis example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0154] [Slurry Preparation Example 4]
[0155] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in synthesis example 5 (HBA / CEA=60 / 40, Na salt, weight average molecular weight 840000, non-volatile component concentration 14.9%) is used instead of synthesis example 1, and 3.73 weight parts of the aqueous latex resin (Y) synthesized in synthesis example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0156] [Slurry Preparation Example 5]
[0157] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in Synthesis Example 7 (HEA / AA / AAM=60 / 30 / 10, Na salt, weight average molecular weight 730,000, non-volatile component concentration 15.1%) is used instead of Synthesis Example 1, and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0158] [Slurry Preparation Example 6]
[0159] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in synthesis example 8 (HEA / AA / AAM=20 / 20 / 60, ammonium salt, weight average molecular weight 780,000, non-volatile component concentration 15.0%) is used instead of synthesis example 1, and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in synthesis example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0160] [Slurry Preparation Example 7]
[0161] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in synthesis example 11 (HEA / AA / HAAM=20 / 20 / 60, ammonium salt, weight average molecular weight 830000, non-volatile component concentration 15.0%) is used instead of synthesis example 1, and 3.73 weight parts of the water-based latex resin (Y) synthesized in synthesis example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0162] [Slurry Preparation Example 8]
[0163] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in Synthesis Example 12 (HEA / AA / AAM=10 / 10 / 80, ammonium salt, weight average molecular weight 860,000, non-volatile component concentration 14.9%) is used instead of Synthesis Example 1, and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0164] [Slurry Preparation Example 9]
[0165] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in Synthesis Example 13 (HEA / AA / AAM=35 / 35 / 30, ammonium salt, weight average molecular weight 840,000, non-volatile component concentration 15.0%) is used instead of Synthesis Example 1, and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0166] [Slurry Preparation Example 10]
[0167] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in Synthesis Example 14 (HEA / AA / AAM=20 / 40 / 40, ammonium salt, weight average molecular weight 830,000, non-volatile component concentration 15.1%) is used instead of Synthesis Example 1, and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0168] [Slurry Preparation Example 11]
[0169] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in Synthesis Example 15 (HEA / AA / AAM=30 / 20 / 50, ammonium salt, weight average molecular weight 840,000, non-volatile component concentration 15.1%) is used instead of Synthesis Example 1, and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0170] [Slurry Preparation Example 12]
[0171] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in Synthesis Example 8 (HEA / AA / AAM=20 / 20 / 60, ammonium salt, weight average molecular weight 780,000, non-volatile component concentration 15.0%) is used instead of Synthesis Example 1, and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 19 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0172] [Slurry Preparation Example 13]
[0173] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in Synthesis Example 8 (HEA / AA / AAM=20 / 20 / 60, ammonium salt, weight average molecular weight 780,000, non-volatile component concentration 15.0%) is used instead of Synthesis Example 1, and 3.70 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 19 (ST / BA / HEMA / MMA / AAM / GMA=34.5 / 50 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.5%) is used instead of SBR.
[0174] [Slurry Preparation Example 14]
[0175] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in Synthesis Example 8 (HEA / AA / AAM=20 / 20 / 60, ammonium salt, weight average molecular weight 780,000, non-volatile component concentration 15.0%) is used instead of Synthesis Example 1, and 3.75 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 20 (BNA / BA / HEMA / MMA / AAM / GMA=34.5 / 50 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.0%) is used instead of SBR.
[0176] [Slurry Preparation Example 15]
[0177] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in Synthesis Example 9 (HEA / AA / AAM=20 / 20 / 60, Li salt, weight average molecular weight 780,000, non-volatile component concentration 15.0%) is used instead of Synthesis Example 1, and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0178] [Slurry Preparation Example 16]
[0179] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in Synthesis Example 10 (HEA / AA / AAM=20 / 20 / 60, Na salt, weight average molecular weight 780,000, non-volatile component concentration 15.0%) is used instead of Synthesis Example 1, and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0180] [Slurry Preparation Example 17]
[0181] 95.0 parts by weight of artificial graphite (initial charge capacity 390 mAh / g, initial discharge capacity 350 mAh / g) and 1.0 parts by weight of acetylene black were weighed and stirred for 30 seconds using a rotation-revolution mixer (ARE-310 manufactured by Thinky Co., Ltd.) at a rotation of 1000 rpm and a revolution of 2000 rpm. 39.5 parts by weight (1.58 parts by weight in terms of solid content conversion weight) of an aqueous solution prepared by diluting the binder composition (HEA / AA / AAM=20 / 20 / 60, ammonium salt, weight average molecular weight 780000, non-volatile component concentration 15.0%) prepared in Synthesis Example 8 above with distilled water to adjust the non-volatile component concentration to 4.0% and 12.5 parts by weight of distilled water were added and mixed until the whole became a paste. Next, the mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm in a rotation and revolution mixer (ARE-310 manufactured by Thinky). Heat was released by stirring, so the mixture was cooled to room temperature with ice water. The mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm, and then cooled to room temperature with ice water. 10.5 parts by weight (0.42 parts by weight in terms of non-volatile component conversion) of an aqueous solution of the adhesive composition shown in Synthesis Example 8 prepared previously to have a non-volatile component concentration of 4% was added, and mixed until the whole mixture became uniform. The mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm in a rotation and revolution mixer (ARE-310 manufactured by Thinky), and then cooled to room temperature with ice water. Add 6 parts by weight of distilled water and 4.98 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%), and use a rotation / revolution mixer (ARE-310 manufactured by Thinky) to stir for 30 seconds at a rotation of 1000 rpm and a revolution of 2000 rpm to prepare a negative electrode mixture slurry.
[0182] [Slurry Preparation Example 18]
[0183] 96.0 parts by weight of artificial graphite (initial charge capacity 390 mAh / g, initial discharge capacity 350 mAh / g) and 1.0 parts by weight of acetylene black were weighed and stirred for 30 seconds using a rotation-revolution mixer (ARE-310 manufactured by Thinky Co., Ltd.) at a rotation of 1000 rpm and a revolution of 2000 rpm. 19.5 parts by weight (0.78 parts by weight in terms of solid content conversion weight) of an aqueous solution prepared by diluting the binder composition (HEA / AA / AAM=20 / 20 / 60, ammonium salt, weight average molecular weight 780000, non-volatile component concentration 15.0%) prepared in Synthesis Example 8 above with distilled water to adjust the non-volatile component concentration to 4.0% and 32.5 parts by weight of distilled water were added and mixed until the whole became a paste. Next, the mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm in a rotation and revolution mixer (ARE-310 manufactured by Thinky). Heat was released by stirring, so the mixture was cooled to room temperature with ice water. The mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm, and then cooled to room temperature with ice water. 10.5 parts by weight (0.42 parts by weight in terms of non-volatile component conversion) of an aqueous solution of the adhesive composition shown in Synthesis Example 8 prepared previously to have a non-volatile component concentration of 4% was added, and mixed until the whole mixture became uniform. The mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm in a rotation and revolution mixer (ARE-310 manufactured by Thinky), and then cooled to room temperature with ice water. Add 6 parts by weight of distilled water and 2.99 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%), and use a rotation / revolution mixer (ARE-310 manufactured by Thinky) to stir for 30 seconds at a rotation of 1000 rpm and a revolution of 2000 rpm to prepare a negative electrode mixture slurry.
[0184] [Slurry Preparation Example 19]
[0185] 3.7 parts by weight of SiO negative electrode material (initial charge capacity 2062 mAh / g, initial discharge capacity 1631 mAh / g), 92.3 parts by weight of artificial graphite (initial charge capacity 390 mAh / g, initial discharge capacity 350 mAh / g), and 1.0 parts by weight of acetylene black were weighed and stirred for 30 seconds using a rotation-revolution mixer (ARE-310 manufactured by Thinky Co., Ltd.) at a rotation of 1000 rpm and a revolution of 2000 rpm. 27.0 parts by weight (1.08 parts by weight in terms of solid content conversion weight) of an aqueous solution prepared by dissolving the binder composition (HEA / AA / AAM=20 / 20 / 60, ammonium salt, weight average molecular weight 780000, non-volatile content concentration 15.0%) prepared in Synthesis Example 8 above in distilled water and adjusting the non-volatile content concentration to 4.0% were added, and 21.0 parts by weight of distilled water were mixed until the whole became a paste. Next, the mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm in a rotation and revolution mixer (ARE-310 manufactured by Thinky). Heat was released by stirring, so the mixture was cooled to room temperature with ice water. The mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm, and then cooled to room temperature with ice water. 10.5 parts by weight (0.42 parts by weight in terms of non-volatile component conversion) of an aqueous solution of the adhesive composition synthesized in Synthesis Example 8 prepared previously to a non-volatile component concentration of 4% was added, and mixed until the whole mixture became uniform. The mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm in a rotation and revolution mixer (ARE-310 manufactured by Thinky), and then cooled to room temperature with ice water. Add 7 parts by weight of distilled water and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%), and use a rotation / revolution mixer (ARE-310 manufactured by Thinky) to stir for 30 seconds at a rotation of 1000 rpm and a revolution of 2000 rpm to prepare a negative electrode mixture slurry.
[0186] [Slurry Preparation Example 20]
[0187] The negative electrode mixture slurry was prepared in the same manner as in slurry preparation example 19 except for using 5.3 weight parts of SiO negative electrode material (first charge capacity 2062 mAh / g, first discharge capacity 1631 mAh / g) and 90.7 weight parts of artificial graphite (first charge capacity 390 mAh / g, first discharge capacity 350 mAh / g).
[0188] [Slurry Preparation Example 21]
[0189] 96.0 parts by weight of artificial graphite (initial charge capacity 390 mAh / g, initial discharge capacity 350 mAh / g) and 1.0 parts by weight of acetylene black were weighed and stirred for 30 seconds using a rotation-revolution mixer (ARE-310 manufactured by Thinky Co., Ltd.) at a rotation of 1000 rpm and a revolution of 2000 rpm. 48.0 parts by weight (0.96 parts by weight in terms of solid content conversion weight) of an aqueous solution prepared by dissolving carboxymethyl cellulose sodium salt (CMC, SUNROSEMAC350HC manufactured by Nippon Paper Industries, Ltd.) in distilled water and adjusting the non-volatile component concentration to 2.0% were added and mixed until the whole became a paste. Next, the mixture was stirred for 2 minutes using a rotation-revolution mixer (ARE-310 manufactured by Thinky Co., Ltd.) at a rotation of 1000 rpm and a revolution of 2000 rpm. Heat was released due to stirring, so the mixture was cooled to room temperature using ice water. After stirring for 2 minutes under the conditions of rotation of 1000 rpm and revolution of 2000 rpm, the mixture was cooled to room temperature with ice water. 27.0 parts by weight of the aqueous solution of CMC prepared previously to a non-volatile component concentration of 2% (0.54 parts by weight in terms of non-volatile component conversion weight) was added and mixed until the whole became uniform. Then, the mixture was stirred for 2 minutes under the conditions of rotation of 1000 rpm and revolution of 2000 rpm using a rotation and revolution mixer (ARE-310 manufactured by Thinky Co., Ltd.), and cooled to room temperature with ice water. 20 parts by weight of distilled water and 2.95 parts by weight of styrene butadiene copolymer (SBR) (DS407H manufactured by DIC Co., Ltd., non-volatile component concentration of 50.8%) were added, and the mixture was stirred for 30 seconds under the conditions of rotation of 1000 rpm and revolution of 2000 rpm using a rotation and revolution mixer (ARE-310 manufactured by Thinky Co., Ltd.), thereby preparing a negative electrode mixture slurry.
[0190] [Slurry Preparation Example 22]
[0191] 96.0 parts by weight of artificial graphite (initial charge capacity 390 mAh / g, initial discharge capacity 350 mAh / g) and 1.0 parts by weight of acetylene black were weighed and stirred for 30 seconds using a rotation-revolution mixer (ARE-310 manufactured by Thinky Co., Ltd.) at a rotation of 1000 rpm and a revolution of 2000 rpm. 27.0 parts by weight (2.16 parts by weight in terms of solid content conversion weight) of an aqueous solution prepared by diluting the binder composition (HEA / AA=60 / 40, Na salt, weight average molecular weight 850000, non-volatile component concentration 14.8%) synthesized in Synthesis Example 1 above and adjusting the non-volatile component concentration to 8.0% and 21.0 parts by weight of distilled water were added and mixed until the whole became a paste. Next, the mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm in a rotation and revolution mixer (ARE-310 manufactured by Thinky). Heat was released by stirring, so the mixture was cooled to room temperature with ice water. The mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm, and then cooled to room temperature with ice water. 10.5 parts by weight (0.84 parts by weight in terms of non-volatile component conversion) of an aqueous solution of the adhesive composition synthesized in Synthesis Example 7, which was previously prepared to have a non-volatile component concentration of 8.0%, was added and mixed until the whole mixture became uniform. The mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm in a rotation and revolution mixer (ARE-310 manufactured by Thinky), and then cooled to room temperature with ice water. 7 parts by weight of distilled water was added, and the mixture was stirred again for 30 seconds using a rotation / revolution mixer (ARE-310 manufactured by Thinky) at a rotation speed of 1000 rpm and a revolution speed of 2000 rpm to prepare a negative electrode mixture slurry.
[0192] [Slurry Preparation Example 23]
[0193] A negative electrode mixture slurry was prepared in the same manner as in slurry preparation example 21, except that 3.73 parts by weight of the aqueous latex resin (Y) (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile matter concentration 40.2%) synthesized in synthesis example 18 was used instead of SBR.
[0194] [Slurry Preparation Example 24]
[0195] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in synthesis example 2 (HBA / AA=60 / 40, Na salt, weight average molecular weight 480,000, non-volatile component concentration 15.0%) is used instead of synthesis example 1, and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in synthesis example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0196] [Slurry Preparation Example 25]
[0197] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in synthesis example 3 (HBA / AA=75 / 35, Na salt, weight average molecular weight 750,000, non-volatile component concentration 14.9%) is used instead of synthesis example 1, and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in synthesis example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0198] [Slurry Preparation Example 26]
[0199] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in Synthesis Example 6 (HBA / AA=60 / 40, unneutralized, weight average molecular weight 830,000, non-volatile component concentration 15.0%) is used instead of Synthesis Example 1, and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0200] [Slurry Preparation Example 27]
[0201] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in Synthesis Example 16 (HEA / AAM=70 / 30, Na salt, weight average molecular weight 750,000, non-volatile component concentration 15.0%) is used instead of Synthesis Example 1, and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0202] [Slurry Preparation Example 28]
[0203] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that the binder composition synthesized in Synthesis Example 17 (AA / AAM=70 / 30, Na salt, weight average molecular weight 820000, non-volatile component concentration 15.0%) is used instead of Synthesis Example 1, and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration 40.2%) is used instead of SBR.
[0204] [Slurry Preparation Example 29]
[0205] A negative electrode mixture slurry is prepared in the same manner as in slurry preparation example 1, except that polyacrylic acid sodium salt (manufactured by Wako Pure Chemical Industries, Ltd., with a degree of polymerization of 22,000 to 70,000) is used instead of Synthesis Example 1, and 3.73 parts by weight of the aqueous latex resin (Y) synthesized in Synthesis Example 18 (ST / BA / HEMA / MMA / AAM / GMA=54.5 / 30 / 8 / 5 / 2 / 0.5, non-volatile component concentration of 40.2%) is used instead of SBR.
[0206] [Slurry Preparation Example 30]
[0207] Weigh 95.0 parts by weight of artificial graphite (initial charge capacity 390 mAh / g, initial discharge capacity 350 mAh / g), 1.0 parts by weight of acetylene black, and 2.0 parts by weight of carboxymethyl cellulose Na salt (CMC, SUNROSE MAC350HC manufactured by Nippon Paper Manufacturing Co., Ltd.), and stir for 30 seconds using a self-rotation and revolution mixer (ARE-310 manufactured by Thinky Co., Ltd.) at a rotation of 1000 rpm and a revolution of 2000 rpm. Add 48.0 parts by weight of distilled water and mix until the whole becomes a paste. Next, stir for 2 minutes using a self-rotation and revolution mixer (ARE-310 manufactured by Thinky Co., Ltd.) at a rotation of 1000 rpm and a revolution of 2000 rpm. Heat is released due to stirring, so ice water is used to cool to room temperature. Stir again for 2 minutes at a rotation of 1000 rpm and a revolution of 2000 rpm, and then cool to room temperature using ice water. 10.5 parts by weight of distilled water was added and mixed until the whole became uniform, and then stirred for 2 minutes using a rotation and revolution mixer (ARE-310 manufactured by Thinky) at a rotation of 1000 rpm and a revolution of 2000 rpm, and cooled to room temperature with ice water. 25 parts by weight of distilled water and 3.94 parts by weight of styrene butadiene copolymer (SBR) (DS407H manufactured by DIC, non-volatile component concentration 50.8%) were added, and stirred for 30 seconds using a rotation and revolution mixer (ARE-310 manufactured by Thinky) at a rotation of 1000 rpm and a revolution of 2000 rpm, thereby preparing a negative electrode mixture slurry.
[0208] [Slurry Preparation Example 31]
[0209] Weigh 96.6 parts by weight of artificial graphite (initial charge capacity 390 mAh / g, initial discharge capacity 350 mAh / g), 1.0 parts by weight of acetylene black, and 1.2 parts by weight of carboxymethyl cellulose Na salt (CMC, SUNROSE MAC350HC manufactured by Nippon Paper Manufacturing Co., Ltd.), and stir for 30 seconds using a self-rotation and revolution mixer (ARE-310 manufactured by Thinky Co., Ltd.) at a rotation of 1000 rpm and a revolution of 2000 rpm. Add 48.0 parts by weight of distilled water and mix until the whole becomes a paste. Next, stir for 2 minutes using a self-rotation and revolution mixer (ARE-310 manufactured by Thinky Co., Ltd.) at a rotation of 1000 rpm and a revolution of 2000 rpm. Heat is released due to stirring, so ice water is used to cool to room temperature. Stir again for 2 minutes at a rotation of 1000 rpm and a revolution of 2000 rpm, and then cool to room temperature using ice water. 10.5 parts by weight of distilled water (0.42 parts by weight in terms of non-volatile content) was added and mixed until the whole was uniform, then stirred for 2 minutes using a rotary mixer (ARE-310 manufactured by Thinky) at 1000 rpm and 2000 rpm, and cooled to room temperature with ice water. 20 parts by weight of distilled water and 2.36 parts by weight of styrene-butadiene copolymer (SBR) (DS407H manufactured by DIC, non-volatile content concentration 50.8%) were added, and stirred for 30 seconds using a rotary mixer (ARE-310 manufactured by Thinky) at 1000 rpm and 2000 rpm, thereby preparing a negative electrode mixture slurry.
[0210] [Slurry Preparation Example 32]
[0211] 3.7 parts by weight of SiO negative electrode material (initial charge capacity 2062 mAh / g, initial discharge capacity 1631 mAh / g), 92.3 parts by weight of artificial graphite (initial charge capacity 390 mAh / g, initial discharge capacity 350 mAh / g), and 1.0 parts by weight of acetylene black were weighed and stirred for 30 seconds using a rotation-revolution mixer (ARE-310 manufactured by Thinky Co., Ltd.) at a rotation of 1000 rpm and a revolution of 2000 rpm. 48.0 parts by weight (0.96 parts by weight in terms of solid content conversion weight) of an aqueous solution prepared by dissolving carboxymethyl cellulose sodium salt (CMC, SUNROSE MAC350HC manufactured by Nippon Paper Industries, Ltd.) in distilled water and adjusting the non-volatile component concentration to 2.0% were added and mixed until the whole became a paste. Next, the mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm in a rotation and revolution mixer (ARE-310 manufactured by Thinky Co.). Since heat was released by stirring, the mixture was cooled to room temperature with ice water. The mixture was stirred again for 2 minutes at 1000 rpm and 2000 rpm, and then cooled to room temperature with ice water. 27.0 parts by weight of the aqueous solution of CMC prepared to have a non-volatile component concentration of 2% (0.54 parts by weight in terms of non-volatile component conversion weight) was added and mixed until the whole mixture became uniform. The mixture was stirred for 2 minutes at 1000 rpm and 2000 rpm in a rotation and revolution mixer (ARE-310 manufactured by Thinky Co.), and then cooled to room temperature with ice water. Add 20 parts by weight of distilled water and 2.95 parts by weight of styrene-butadiene copolymer (SBR) (DS407H manufactured by DIC, non-volatile component concentration 50.8%), and stir again for 30 seconds using a rotation / revolution mixer (ARE-310 manufactured by Thinky) at a rotation of 1000 rpm and a revolution of 2000 rpm to prepare a negative electrode mixture slurry.
[0212] [Slurry Preparation Example 33]
[0213] The negative electrode mixture slurry was prepared in the same manner as in slurry preparation example 32 except for using 5.3 weight parts of SiO negative electrode material (first charge capacity 2062 mAh / g, first discharge capacity 1631 mAh / g) and 91.3 weight parts of artificial graphite (first charge capacity 390 mAh / g, first discharge capacity 350 mAh / g).
[0214] “Production of negative electrode”
[0215] [Example 1]
[0216] The negative electrode mixture coating amount (surface density) after drying was 13.2 mg / cm 2The gap of the rod coater was adjusted in a manner, and the negative electrode mixture slurry prepared in Slurry Preparation Example 1 was applied to the electrolytic copper foil (thickness 10 μm, width 180 mm) as the collector by the rod coater. Thereafter, it was dried for 8 minutes in an air-supplied dryer set at 80°C. The dried electrode was cut into short strips of 40 mm in width and pressed using a roller press (small tabletop roller press SA-602 manufactured by TESTER SANGYO CO,.LTD.) until the mixture layer density became 1.70 g / cm 3 After vacuum drying at 110°C for 10 hours, the density of the mixed layer was measured again and found to be 1.65 g / cm 3 (The thickness of the mixture layer was 80.0 μm). The initial charge capacity per unit area of the electrode was 4.97 mAh / cm 2 Thus, the negative electrode of Example 1 (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 ).
[0217] (Measurement of peel strength and confirmation of electrode winding resistance)
[0218] After the negative electrode prepared above was placed in a constant temperature and humidity chamber at a temperature of 25°C and a relative humidity of 50% for 6 hours, it was cut into short strips of 25 mm wide and 100 mm long. Next, a double-sided tape (Nο5015 manufactured by Nitto Denko Corporation) was used to adhere the active material surface to a stainless steel plate as the adhered surface to prepare a sample for a peel strength test. The copper foil end was peeled off by about 10 mm, and a polyimide tape was attached thereto to prepare a mounting portion for mounting on a peel tester. The sample for the peel strength test was mounted on a peel tester (Autograph AG-X Plus manufactured by Shimadzu Corporation), and a 180-degree peel test was performed. The peel strength was 34.5 N / m. Next, the peeling (destruction) state of the negative electrode coating was observed. In addition, the negative electrode coating was wound on a φ5 mm core, and the coating was visually observed to see if cracks occurred. At this time, no cracks occurred.
[0219] [Example 2]
[0220] The negative electrode (surface density 13.2 gm / cm) of Example 2 was prepared in the same manner as Example 1 except that the negative electrode mixture slurry shown in Example 2 was used. 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 31.5 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0221] [Example 3]
[0222] The negative electrode (surface density 13.2 gm / cm) of Example 3 was prepared in the same manner as Example 1 except that the negative electrode mixture slurry shown in Example 3 was used. 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 27.8 N / m. Furthermore, when the film was wound on a core of φ5 mm, no cracks were generated.
[0223] [Example 4]
[0224] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 28.9 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0225] [Example 5]
[0226] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3The peel strength at this time was 28.9 N / m. Furthermore, when the film was wound on a core of φ5 mm, no cracks were generated.
[0227] [Example 6]
[0228] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 30.7 N / m. Furthermore, when the film was wound on a core of φ5 mm, no cracks were generated.
[0229] [Example 7]
[0230] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 28.4 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0231] [Example 8]
[0232] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 29.1 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0233] [Example 9]
[0234] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 30.5 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0235] [Example 10]
[0236] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 28.6 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0237] [Example 11]
[0238] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 28.6 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0239] [Example 12]
[0240] A negative electrode (surface density 13.2 gm / cm 2, density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 30.1 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0241] [Example 13]
[0242] A negative electrode (surface density 13.2 gm / cm) was prepared in the same manner as in Example 1 except that the negative electrode mixture slurry shown in the slurry preparation example 13 was used. 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 32 N / m. Furthermore, when the film was wound on a core of φ5 mm, no cracks were generated.
[0243] [Example 14]
[0244] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 29.8 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0245] [Example 15]
[0246] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 29.5 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0247] [Example 16]
[0248] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 34.6 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0249] [Example 17]
[0250] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.89mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 56.0 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0251] [Example 18]
[0252] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3The peel strength at this time was 16.2 N / m. Furthermore, when the film was wound on a core of φ5 mm, no cracks were generated.
[0253] [Example 19]
[0254] The electrode density after vacuum drying using the negative electrode mixture slurry shown in the slurry preparation example 6 was 1.40 g / cm 3 A negative electrode (surface density 13.2 gm / cm) was prepared in the same manner as in Example 1 except that the pressure of the roller press was appropriately adjusted (the thickness of the mixture layer was 94.3 μm). 2 , density of composite layer 1.40g / cm 3 , mixture layer thickness 94.3μm, first charge capacity per unit area 4.97mAh / cm 2 ). The peel strength at this time was 29.0 N / m. In addition, when it was wound on a core of φ5 mm, no cracks occurred.
[0255] [Example 20]
[0256] The electrode density after vacuum drying using the negative electrode mixture slurry shown in the slurry preparation example 6 was 1.75 g / cm 3 A negative electrode (surface density 13.2 gm / cm) was prepared in the same manner as in Example 1 except that the pressure of the roller press was appropriately adjusted (the thickness of the mixture layer was 75.4 μm). 2 , the density of the composite layer is 1.75g / cm 3 , mixture layer thickness 75.4μm, first charge capacity per unit area 4.97mAh / cm 2 ). The peel strength at this time was 35.2 N / m. In addition, when it was wound on a core of φ5 mm, no cracks occurred.
[0257] [Example 21]
[0258] The negative electrode mixture slurry shown in the above slurry preparation example 6 was used and the negative electrode mixture coating amount (surface density) was 18.2 mg / cm 2 A negative electrode (surface density 18.2 gm / cm) was prepared in the same manner as in Example 1 except that the gap of the rod coater was adjusted by 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 110.0μm, first charge capacity per unit area 6.81mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3The peel strength at this time was 30.1 N / m. Furthermore, when the film was wound on a core of φ5 mm, no cracks occurred.
[0259] [Example 22]
[0260] The negative electrode mixture slurry shown in the above slurry preparation example 6 was used and the negative electrode mixture coating amount (surface density) was 20.7 mg / cm 2 A negative electrode (surface density 20.7 gm / cm) was prepared in the same manner as in Example 1 except that the gap of the rod coater was adjusted by 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 125.5μm, first charge capacity per unit area 7.75mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength was 25.5 N / m. When the film was wound on a core of φ5 mm, no cracks were generated.
[0261] [Example 23]
[0262] The negative electrode mixture slurry shown in the above slurry preparation example 19 was used and the negative electrode mixture coating amount (surface density) was 11.3 mg / cm 2 The gap of the bar coater was adjusted in such a way that the electrode density after vacuum drying became 1.65 g / cm 3 A negative electrode (surface density 11.3 gm / cm) was prepared in the same manner as in Example 1 except that the pressure of the roller press was appropriately adjusted (the thickness of the mixture layer was 68.5 μm). 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 68.5μm, first charge capacity per unit area 4.94mAh / cm 2 ). The peel strength at this time was 32.0 N / m. In addition, when it was wound on a core of φ5 mm, no cracks occurred.
[0263] [Example 24]
[0264] The negative electrode mixture slurry shown in the above slurry preparation example 20 was used and the negative electrode mixture coating amount (surface density) was 10.7 mg / cm 2 The gap of the bar coater was adjusted in such a way that the electrode density after vacuum drying became 1.65 g / cm 3 A negative electrode (surface density 10.7 gm / cm) was prepared in the same manner as in Example 1 except that the pressure of the roller press was appropriately adjusted (the thickness of the mixture layer was 64.8 μm).2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 64.8μm, first charge capacity per unit area 4.98mAh / cm 2 ). The peel strength at this time was 34.0 N / m. In addition, when it was wound around a core of φ5 mm, no cracks occurred.
[0265] [Comparative Example 1]
[0266] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 16.8 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0267] [Comparative Example 2]
[0268] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 38.0 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0269] [Comparative Example 3]
[0270] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3The peel strength at this time was 14.8 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0271] [Comparative Example 4]
[0272] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 17.4 N / m. Furthermore, when the film was wound on a core of φ5 mm, no cracks were generated.
[0273] [Comparative Example 5]
[0274] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 14.5 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0275] [Comparative Example 6]
[0276] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 18.0 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0277] [Comparative Example 7]
[0278] Except for the above slurry, Example 27 (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 ) were used to prepare the negative electrode in the same manner as in Example 1. The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 15.2 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0279] [Comparative Example 8]
[0280] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 14.5 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0281] [Comparative Example 9]
[0282] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 16.4 N / m. Furthermore, when the film was wound on a core of φ5 mm, no cracks were generated.
[0283] [Comparative Example 10]
[0284] A negative electrode (surface density 13.2 gm / cm 2, density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.89mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 56.0 N / m. Furthermore, when the film was wound around a core of φ5 mm, no cracks were generated.
[0285] [Comparative Example 11]
[0286] A negative electrode (surface density 13.2 gm / cm 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 80.0μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 16.2 N / m. Furthermore, when the film was wound on a core of φ5 mm, no cracks were generated.
[0287] [Comparative Example 12]
[0288] The electrode density after vacuum drying using the negative electrode mixture slurry shown in the slurry preparation example 21 was 1.40 g / cm 3 A negative electrode (surface density 13.2 gm / cm) was prepared in the same manner as in Example 1 except that the pressure of the roller press was appropriately adjusted (the thickness of the mixture layer was 94.3 μm). 2 , density of composite layer 1.40g / cm 3 , mixture layer thickness 94.3μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.40 g / cm 3 The peel strength at this time was 14.6 N / m. Furthermore, when the film was wound on a core of φ5 mm, no cracks were generated.
[0289] [Comparative Example 13]
[0290] The electrode density after vacuum drying using the negative electrode mixture slurry shown in the slurry preparation example 21 was 1.75 g / cm 3A negative electrode (surface density 13.2 gm / cm) was prepared in the same manner as in Example 1 except that the pressure of the roller press was appropriately adjusted (the thickness of the mixture layer was 75.4 μm). 2 , the density of the composite layer is 1.75g / cm 3 , mixture layer thickness 75.4μm, first charge capacity per unit area 4.97mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.75 g / cm 3 The peel strength at this time was 18.2 N / m. Furthermore, when the film was wound on a core of φ5 mm, no cracks were generated.
[0291] [Comparative Example 14]
[0292] The negative electrode mixture slurry shown in the above slurry preparation example 21 was used and the negative electrode mixture coating amount (surface density) was 18.2 mg / cm 2 A negative electrode (surface density 18.2 gm / cm) was prepared in the same manner as in Example 1 except that the gap of the rod coater was adjusted by 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 110.0μm, first charge capacity per unit area 6.18mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength at this time was 20.0 N / m. Furthermore, when the film was wound on a core of φ5 mm, no cracks were generated.
[0293] [Comparative Example 15]
[0294] The negative electrode mixture slurry shown in the above slurry preparation example 21 was used and the negative electrode mixture coating amount (surface density) was 20.7 mg / cm 2 A negative electrode (surface density 20.7 gm / cm) was prepared in the same manner as in Example 1 except that the gap of the rod coater was adjusted by 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 125.5μm, first charge capacity per unit area 7.75mAh / cm 2 The pressure of the roller press was such that the density of the mixture layer after vacuum drying became 1.65 g / cm 3 The peel strength was 13.2 N / m. When the film was wound on a core of φ5 mm, no cracks were generated.
[0295] [Comparative Example 16]
[0296] The negative electrode mixture slurry shown in the above slurry preparation example 30 was used and the negative electrode mixture coating amount (surface density) was 11.3 mg / cm 2 The gap of the bar coater was adjusted in such a way that the electrode density after vacuum drying became 1.65 g / cm 3 A negative electrode (surface density 11.3 gm / cm) was prepared in the same manner as in Example 1 except that the pressure of the roller press was appropriately adjusted (the thickness of the mixture layer was 68.5 μm). 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 68.5μm, first charge capacity per unit area 4.94mAh / cm 2 ). The peel strength at this time was 20.3 N / m. In addition, when it was wound on a core of φ5 mm, no cracks occurred.
[0297] [Comparative Example 17]
[0298] The negative electrode mixture slurry shown in the above slurry preparation example 31 was used and the negative electrode mixture coating amount (surface density) was 10.7 mg / cm 2 The gap of the bar coater was adjusted in such a way that the electrode density after vacuum drying became 1.65 g / cm 3 A negative electrode (surface density 10.7 gm / cm) was prepared in the same manner as in Example 1 except that the pressure of the roller press was appropriately adjusted (the thickness of the mixture layer was 64.8 μm). 2 , density of composite layer 1.65g / cm 3 , mixture layer thickness 64.8μm, first charge capacity per unit area 4.98mAh / cm 2 ). The peel strength at this time was 22.5 N / m. In addition, when it was wound on a core of φ5 mm, no cracks occurred.
[0299] “Making the positive electrode”
[0300] “Preparation of positive electrode mixture slurry”
[0301] The positive electrode material LiMn 0.6 Co 0.2 Ni 0.2 O 2 94.0 parts by weight of (initial charge capacity 191 mAh / g, initial discharge capacity 171 mAh / g), 3.0 parts by weight of acetylene black, and 3.0 parts by weight of polyvinylidene fluoride were dispersed in N-methyl-2-pyrrolidone to form a positive electrode mixture slurry. Furthermore, the non-volatile component in the positive electrode mixture slurry was 50 parts by weight relative to the total mass of the slurry.
[0302] Weigh the positive electrode material LiMn 0.6Co 0.2 Ni 0.2 O 2 94.0 parts by weight of (initial charge capacity 191 mAh / g, initial discharge capacity 171 mAh / g), 3.0 parts by weight of acetylene black are placed in a drying room where the dew point is controlled below -30°C, and stirred for 30 seconds using a self-rotating and revolving mixer (ARE-310 manufactured by Thinky) at a rotation of 1000 rpm and a revolution of 2000 rpm. 30.0 parts by weight (3.0 parts by weight in terms of solid content conversion weight) of a 10% NMP solution of polyvinylidene fluoride (PVDF, #1100 manufactured by KUREHA) are added, and mixed until the whole becomes a paste. Then, a self-rotating and revolving mixer (ARE-310 manufactured by Thinky) is used to stir for 1 minute at a rotation of 1000 rpm and a revolution of 2000 rpm. Heat is released due to stirring, so the mixture is cooled to room temperature. The stirring and cooling operation performed by the self-rotating and revolving mixer is repeated 3 times. Then add 10.0 parts by weight of NMP and mix until the whole becomes uniform. Then stir for 1 minute using a rotation and revolution mixer (ARE-310 manufactured by Thinky) at a rotation of 1000 rpm and a revolution of 2000 rpm. Heat is released due to stirring, so cool to room temperature. The stirring and cooling operation performed by the rotation and revolution mixer is repeated 3 times. Then add 10.0 parts by weight of NMP and stir for 2 minutes using a rotation and revolution mixer (ARE-310 manufactured by Thinky) at a rotation of 1000 rpm and a revolution of 2000 rpm to prepare a positive electrode mixture slurry.
[0303] [Positive Electrode Preparation Example 1]
[0304] "Surface density 25.0mg / cm 2 "Cathode production"
[0305] First, the amount of the mixture applied after drying (surface density) was set to 25.0 mg / cm 2 The gap of the rod coater was adjusted in a manner, and the positive electrode mixture slurry prepared above was applied to the collector aluminum foil (thickness 15μm, width 180mm) as the collector by the rod coater. The positive electrode mixture slurry was then dried for 15 minutes using an air-supplied dryer set at 80°C. Next, the mixture was passed through a roller press until the mixture density became 3.40g / cm 3 Finally, the positive electrode mixture was vacuum dried at 110°C for 10 hours to produce a positive electrode mixture with a surface density of 25.0 mg / cm 2 Positive electrode (surface density 25.0gm / cm 2 , density of composite layer 3.40g / cm3 , mixture layer thickness 73.5μm, first charge capacity per unit area 4.49mAh / cm 2 ).
[0306] [Positive Electrode Preparation Example 2]
[0307] "Surface density 34.2mg / cm 2 "Cathode production"
[0308] Divided by the coating amount (surface density) of the mixture, it becomes 34.2 mg / cm 2 The positive electrode (surface density 34.2 gm / cm) was prepared in the same manner as in Positive Electrode Preparation Example 1 except that the gap of the rod coater was adjusted by 2 , density of composite layer 3.40g / cm 3 , mixture layer thickness 58.4μm, first charge capacity per unit area 6.14mAh / cm 2 ).
[0309] [Positive Electrode Preparation Example 3]
[0310] "Surface density 39.2mg / cm 2 "Cathode production"
[0311] Divided by the coating amount (surface density) of the mixture, it becomes 39.2 mg / cm 2 The positive electrode (surface density 39.2 gm / cm) was prepared in the same manner as in Positive Electrode Preparation Example 1 except that the gap of the rod coater was adjusted by 2 , density of composite layer 3.40g / cm 3 , mixture layer thickness 68.0μm, first charge capacity per unit area 7.04mAh / cm 2 ).
[0312] "Battery Production"
[0313] [Example 25]
[0314] Use a Thomson knife to cut the negative electrode shown in Example 1 into a 24mm×24mm square with a tap (Tab), and cut the positive electrode shown in Positive Electrode Preparation Example 1 into a 22mm×22mm square with a tap. The nickel tab leads of the negative electrode and the aluminum tab leads of the positive electrode are respectively welded to the tap parts of the cut electrodes. Next, use a Thomson knife to cut the diaphragm (polyethylene microporous film with a thickness of 20 microns) into a 28mm×38mm rectangle. The positive electrode and the negative electrode are placed opposite each other through the diaphragm, packaged with a laminated film, and the tap parts are fixed by thermal compression. Next, add the electrolyte (1.0M LiPF 6300 μL of a mixed solution of ethylene carbonate / dimethyl carbonate / ethyl methyl carbonate = 30 / 30 / 40 (volume ratio) + 1% ethylene carbonate + 5% fluoroethylene carbonate) was added and sealed by vacuum lamination to prepare a laminated secondary battery.
[0315] (First charge and discharge (chemical conversion treatment))
[0316] The secondary battery was sandwiched between two GORE Hyper-Sheets, and then clamped with two acrylic plates, and fixed with two long tail clips to evenly apply fixed pressure to the electrode parts. It was installed in a charge and discharge device, placed at 25°C for 3 hours, and then charged and discharged once at a charge and discharge rate of 0.1C. The first charge and discharge efficiency at this time was 84.6%.
[0317] (Electrode expansion measurement)
[0318] After the first charge and discharge, the temperature was kept at 45°C, and after charging once at 0.5C, the secondary battery was disassembled in a drying room, and the fully charged negative electrode was taken out. After washing with dimethyl carbonate and natural drying, the electrode thickness was measured with a micrometer, and the thickness of the current collector was subtracted to obtain the thickness of the mixture layer. The electrode mixture layer thickness before charging was set as 100 and the electrode expansion rate was calculated, and the result was 17.5%.
[0319] (45℃ Cycle Characteristics)
[0320] The temperature of the secondary battery after the first charge and discharge was maintained at 45° C., and charge and discharge were repeated 100 times at 0.5 C. When the first discharge capacity at 0.5 C was set to 100%, the discharge capacity retention rate after 100 cycles was 91.8%.
[0321] (-10℃ Cycle Characteristics)
[0322] The temperature of the secondary battery after the first charge and discharge was maintained at -10°C, and charge and discharge were repeated 100 times at 0.5 C. When the first discharge capacity at 0.5 C was set as 100%, the discharge capacity retention rate after 50 cycles was 84.9%.
[0323] [Example 26]
[0324] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 2 was used. The initial charge and discharge capacity of the secondary battery obtained was 85.0%, the electrode expansion rate was 16.3%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 93.2%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 85.6%.
[0325] [Example 27]
[0326] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 3 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.9%, the electrode expansion rate was 16.6%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 93.3%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 85.5%.
[0327] [Example 28]
[0328] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 4 was used. The initial charge and discharge capacity of the secondary battery obtained was 84.8%, the electrode expansion rate was 16.5%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 91.7%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 84.8%.
[0329] [Example 29]
[0330] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 5 was used. The initial charge and discharge capacity of the secondary battery obtained was 85.0%, the electrode expansion rate was 17.0%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 91.5%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 84.6%.
[0331] [Example 30]
[0332] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 6 was used. The initial charge and discharge capacity of the secondary battery obtained was 85.0%, the electrode expansion rate was 16.8%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 92.1%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 85.0%.
[0333] [Example 31]
[0334] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 7 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.9%, the electrode expansion rate was 16.4%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 91.8%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 85.2%.
[0335] [Example 32]
[0336] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 8 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.8%, the electrode expansion rate was 16.7%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 91.5%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 84.9%.
[0337] [Example 33]
[0338] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 9 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.8%, the electrode expansion rate was 16.4%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 91.7%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 85.0%.
[0339] [Example 34]
[0340] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 10 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.9%, the electrode expansion rate was 16.3%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 91.5%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 83.9%.
[0341] [Example 35]
[0342] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 11 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.8%, the electrode expansion rate was 16.5%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 91.7%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 84.5%.
[0343] [Example 36]
[0344] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 12 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.9%, the electrode expansion rate was 16.6%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 91.8%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 85.2%.
[0345] [Example 37]
[0346] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 13 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.9%, the electrode expansion rate was 16.3%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 91.4%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 84.7%.
[0347] [Example 38]
[0348] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 14 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.9%, the electrode expansion rate was 16.4%, the discharge capacity retention rate after 50 cycles at 45°C and 0.5C was 91.8%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 84.5%.
[0349] [Example 39]
[0350] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 15 was used. The initial charge and discharge capacity of the obtained secondary battery was 86.2%, the electrode expansion rate was 16.7%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 92.1%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 85.4%.
[0351] [Example 40]
[0352] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 16 was used. The initial charge and discharge capacity of the obtained secondary battery was 85.1%, the electrode expansion rate was 16.5%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 92.2%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 85.5%.
[0353] [Example 41]
[0354] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 17 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.9%, the electrode expansion rate was 16.9%, the discharge capacity retention rate after 50 cycles at 45°C and 0.5C was 91.0%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 84.4%.
[0355] [Example 42]
[0356] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 18 was used. The initial charge and discharge capacity of the secondary battery obtained was 84.2%, the electrode expansion rate was 18.2%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 92.4%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 85.7%.
[0357] [Example 43]
[0358] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 19 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.9%, the electrode expansion rate was 16.8%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 93.1%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 86.3%.
[0359] [Example 44]
[0360] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 20 was used. The initial charge and discharge capacity of the secondary battery obtained was 84.8%, the electrode expansion rate was 17.2%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 90.1%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 83.5%.
[0361] [Example 45]
[0362] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 21 and the positive electrode shown in Positive Electrode Preparation Example 2 were used. The initial charge and discharge capacity of the secondary battery obtained was 84.0%, the electrode expansion rate was 19.6%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 88.3%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 81.9%.
[0363] [Example 46]
[0364] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 22 and the positive electrode shown in positive electrode preparation Example 5 were used. The initial charge and discharge capacity of the secondary battery obtained was 83.9%, the electrode expansion rate was 20.1%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 84.2%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 78.1%.
[0365] [Example 47]
[0366] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 23 and the positive electrode shown in Positive Electrode Preparation Example 3 were used. The initial charge and discharge capacity of the secondary battery obtained was 83.2%, the electrode expansion rate was 25.5%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 88.5%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 82.0%.
[0367] [Example 48]
[0368] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Example 24 and the positive electrode shown in Positive Electrode Preparation Example 4 were used. The initial charge and discharge capacity of the secondary battery obtained was 82.9%, the electrode expansion rate was 30.0%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 86.5%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 80.2%.
[0369] [Comparative Example 18]
[0370] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 1 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.5%, the electrode expansion rate was 20.0%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 91.0%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 64.8%.
[0371] [Comparative Example 19]
[0372] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 2 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.2%, the electrode expansion rate was 15.3%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 88.0%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 62.5%.
[0373] [Comparative Example 20]
[0374] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 3 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.3%, the electrode expansion rate was 19.0%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 88.4%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 63.0%.
[0375] [Comparative Example 21]
[0376] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 4 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.8%, the electrode expansion rate was 18.0%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 89.0%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 63.4%.
[0377] [Comparative Example 22]
[0378] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 5 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.3%, the electrode expansion rate was 22.0%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 85.4%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 63.8%.
[0379] [Comparative Example 23]
[0380] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 6 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.9%, the electrode expansion rate was 17.2%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 90.2%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 64.6%.
[0381] [Comparative Example 24]
[0382] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 7 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.7%, the electrode expansion rate was 25.1%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 87.0%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 63.3%.
[0383] [Comparative Example 25]
[0384] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 8 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.6%, the electrode expansion rate was 18.1%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 88.0%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 62.9%.
[0385] [Comparative Example 26]
[0386] The operation was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 9 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.3%, the electrode expansion rate was 20.1%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 86.5%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 64.4%.
[0387] [Comparative Example 27]
[0388] The operation was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 10 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.6%, the electrode expansion rate was 19.8%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 89.6%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 64.4%.
[0389] [Comparative Example 28]
[0390] The process was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 11 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.3%, the electrode expansion rate was 22.0%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 88.3%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 63.8%.
[0391] [Comparative Example 29]
[0392] The operation was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 12 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.8%, the electrode expansion rate was 19.3%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 92.3%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 69.7%.
[0393] [Comparative Example 30]
[0394] The operation was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 13 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.8%, the electrode expansion rate was 21.5%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 89.2%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 67.4%.
[0395] [Comparative Example 31]
[0396] The operation was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 14 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.1%, the electrode expansion rate was 23.5%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 86.1%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 65.1%.
[0397] [Comparative Example 32]
[0398] The operation was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 15 was used. The initial charge and discharge capacity of the obtained secondary battery was 84.0%, the electrode expansion rate was 24.3%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 82.3%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 62.2%.
[0399] [Comparative Example 33]
[0400] The operation was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 16 was used. The initial charge and discharge capacity of the obtained secondary battery was 86.0%, the electrode expansion rate was 30.2%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 82.3%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 65.0%.
[0401] [Comparative Example 34]
[0402] The operation was carried out in the same manner as in Example 25 except that the negative electrode shown in Comparative Example 17 was used. The initial charge and discharge capacity of the obtained secondary battery was 82.8%, the electrode expansion rate was 35.4%, the discharge capacity retention rate after 100 cycles at 45°C and 0.5C was 83.9%, and the discharge capacity retention rate after 50 cycles at -10°C and 0.5C was 63.4%.
[0403] Tables 3 and 4 show the data of the negative electrodes prepared in the above-mentioned synthesis examples, negative electrode slurry preparation examples, positive electrode preparation examples, Examples 1 to 24 and Comparative Examples 1 to 17, and batteries prepared in Examples 25 to 48 and Comparative Examples 18 to 34.
[0404] [Table 3]
[0405]
[0406] [Table 4]
[0407]
[0408] [Table 5]
[0409]
[0410] [Table 6]
[0411]
[0412] As shown in Example 25, when the adhesive uses the water-soluble resin (X) of the present invention comprising a copolymer containing a hydroxyl-containing monomer (a) and an acid-containing monomer (b) as essential components and SBR, the peel strength, the capacity retention rate after 100 cycles at 45°C, and the capacity retention rate after 100 cycles at 0°C are improved compared to the case of using CMC and SBR shown in Comparative Example 1. In addition, as shown in Examples 26 to 28, even when the adhesive uses the water-soluble resin (X) of the present invention comprising a copolymer containing a hydroxyl-containing monomer (a) and an acid-containing monomer (b) as essential components and a latex resin (Y), the peel strength, the capacity retention rate after 100 cycles at 45°C, and the capacity retention rate after 100 cycles at 0°C are improved compared to Comparative Example 1. In addition, as shown in Examples 29 to 38, even when the water-soluble resin (X) further contains other monomers (c), the peel strength, the capacity retention rate after 100 cycles at 45°C, and the capacity retention rate after 100 cycles at 0°C are improved compared to the case of using CMC and SBR shown in Comparative Example 1. These results show that good electrode and battery characteristics can be obtained by using the water-soluble resin (X) of the present invention containing a copolymer containing a hydroxyl group-containing monomer (a) and an acid group-containing monomer (b) as essential components, or a resin in which the water-soluble resin (X) further contains other monomers (c), and the latex resin (Y) as a binder.
[0413] As shown in Examples 38 to 40, even when the acid group-containing monomer (b) is an ammonium salt, a lithium salt, or a sodium salt, the peel strength, the capacity retention rate after 100 cycles at 45°C, and the capacity retention rate after 100 cycles at 0°C are good. These results indicate that even when the acid group-containing monomer (b) is a substance neutralized with an alkaline composition or a light metal hydroxide, good electrode and battery characteristics can be obtained.
[0414] On the other hand, as shown in Comparative Example 17, when the resin (X) of the present invention containing a copolymer having a hydroxyl group-containing monomer (a) and an acid group-containing monomer (b) as essential components is used as a binder without using the aqueous latex (Y), the peel strength is greatly improved compared to the case of using CMC and SBR shown in Comparative Example 1, but the capacity retention rate after 100 cycles at 45°C and the capacity retention rate after 100 cycles at 0°C are reduced. Therefore, it is shown that the use of both the aqueous latex (Y) of the present invention containing a copolymer having a hydroxyl group-containing monomer (a) and an acid group-containing monomer (b) as essential components and the aqueous latex (X) can obtain good electrode and battery characteristics in a single graphite-based negative electrode.
[0415] In addition, as shown in Comparative Example 18, when CMC and the aqueous latex (Y) of the present invention are used, the peel strength, the capacity retention rate after 100 cycles at 45°C, and the capacity retention rate after 100 cycles at 0°C are respectively reduced compared to the case of using CMC and SBR shown in Comparative Example 1. These results show that when the aqueous latex (Y) of the present invention is used in combination with the water-soluble resin (X) of the present invention comprising a copolymer containing a hydroxyl group-containing monomer (a) and an acid group-containing monomer (b) as essential components, good electrode and battery characteristics can be obtained.
[0416] As shown in Examples 30, 43, 44, Comparative Examples 16, 25, and 26, even when the electrode density of the negative electrode is set at 1.40 to 1.75 g / cm 3 In the case of a change in the range of Example 30 (electrode density 1.50 g / cm 3 ), Example 43 (electrode density 1.40 g / cm 3 ), and Example 44 (electrode density 1.75 g / cm 3 ) peel strength, capacity retention rate after 100 cycles at 45°C, and capacity retention rate after 100 cycles at 0°C are also better than those of Comparative Example 16 (electrode density 1.50 g / cm 3 ), Comparative Example 25 (electrode density 1.40 g / cm 3 ), and Comparative Example 26 (electrode density 1.75 g / cm 3 These results show that good electrode and battery characteristics can be obtained by using the water-soluble resin (X) of the present invention comprising a copolymer having a hydroxyl group-containing monomer (a) and an acid group-containing monomer (b) as essential components, a resin further containing other monomers (c), and an aqueous latex (Y).
[0417] As shown in Example 45 and Comparative Example 27 or the above-mentioned Example 46 and Comparative Example 28, even when the negative electrode is thickened, the peel strength, capacity retention rate after 100 cycles at 45°C, and capacity retention rate after 100 cycles at 0°C of Example 45 (negative electrode mixture layer thickness 110 μm) and Example 46 (negative electrode mixture layer thickness 125 μm) are better than those of Comparative Example 27 (negative electrode mixture layer thickness 110 μm) and Comparative Example 28 (negative electrode mixture layer thickness 125 μm) having the same mixture layer thickness. This indicates that even when the negative electrode is thickened, good electrode and battery characteristics can be obtained by using the water-soluble resin (X) of the present invention, which contains a copolymer having a hydroxyl group-containing monomer (a) and an acid group-containing monomer (b) as essential components, and further containing a resin of other monomers (c), and an aqueous latex (Y).
[0418] As shown in Example 47, Comparative Example 48 or Comparative Example 29, and Comparative Example 30, even when a mixed active material of SiO negative electrode material and graphite is used, the peel strength of Example 47 (3.7 parts by weight of SiO negative electrode material) and Example 48 (5.3 parts by weight of SiO negative electrode material), the capacity retention rate after 100 cycles at 45°C, and the capacity retention rate after 100 cycles at 0°C are better than those of Comparative Example 29 (3.7 parts by weight of SiO negative electrode material) and Comparative Example 30 (5.3 parts by weight of SiO negative electrode material) using the same mixed active material. This indicates that even when a mixed active material of SiO negative electrode material and graphite is used as the negative electrode, good electrode and battery characteristics can be obtained by using the water-soluble resin (X) of the present invention, which contains a copolymer having a hydroxyl group-containing monomer (a) and an acid group-containing monomer (b) as essential components, and further contains a resin of other monomers (c), and an aqueous latex (Y).
Claims
1. A negative electrode binder composition comprising a water-soluble resin (X) and an aqueous latex resin (Y), wherein the water-soluble resin (X) comprises a copolymer containing a hydroxyl group-containing monomer (a) and an acid group-containing monomer (b) as essential components, The weight average molecular weight of the copolymer measured using an aqueous GPC measuring device is greater than 700,000, and the swelling rate of a dry film of the copolymer after being immersed in a carbonate-based mixed solvent at 45° C. for 72 hours is 0 to 10% by weight, wherein the carbonate-based mixed solvent is EC, i.e., ethylene carbonate / DEC, i.e., diethylene carbonate = 50 / 50 (wt).
2. The negative electrode binder composition according to claim 1, wherein The hydroxyl-containing monomer (a) is any one or more selected from the group consisting of 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 3-hydroxypropyl acrylate, 2-hydroxybutyl acrylate, 4-hydroxybutyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, and 4-hydroxybutyl methacrylate.
3. The negative electrode binder composition according to claim 1, wherein The acid group-containing monomer (b) is a substance neutralized with an alkaline composition or a light metal salt.
4. The negative electrode binder composition according to claim 1, wherein The acid group-containing monomer (b) is at least one selected from the group consisting of acrylic acid, methacrylic acid, maleic acid, monomethyl maleate, 2-carboxyethyl acrylate, 2-carboxyethyl methacrylate, maleic acid, and itaconic acid.
5. The negative electrode binder composition according to claim 1, wherein The water-soluble resin (X) further contains at least one selected from the group consisting of acrylamide, methacrylamide, N-methylacrylamide, N,N-dimethylacrylamide, and N-methylolacrylamide.
6. The negative electrode binder composition according to claim 1, wherein The total content of the resin components derived from the hydroxyl group-containing monomer (a) and the acid group-containing monomer (b) is 5 to 80% by weight based on the total amount of the water-soluble resin (X).
7. The negative electrode binder composition according to claim 1, wherein The content of any one or more selected from the group consisting of acrylamide, methacrylamide, N-methylacrylamide, N,N-dimethylacrylamide, and N-hydroxymethylacrylamide is 0 to 80% by weight.
8. The negative electrode binder composition according to claim 1, wherein The water-based latex resin (Y) is any one or more of SBR, styrene acrylate copolymer, and acrylate copolymer.
9. The negative electrode binder composition according to claim 8, wherein The styrene acrylate copolymer is butyl acrylate.
10. The negative electrode binder composition according to claim 9, wherein The content of the constituent units derived from the styrene monomer in the total amount of the styrene acrylate copolymer is 40 to 60% by weight, and the content of the constituent units derived from the butyl acrylate monomer is 20 to 40% by weight. 11 . A negative electrode comprising the negative electrode binder composition according to claim 1 as a component.
12. The negative electrode according to claim 11, wherein The total content of the component derived from the water-soluble resin (X) and the component derived from the aqueous latex resin (Y) is 1.5% by weight or more and 5.5% by weight or less.
13. The negative electrode according to claim 11, comprising a graphite-based material as a main active material, and the negative electrode has a volume density of 1.4 g / cm 3 above.
14. The negative electrode according to claim 11, wherein The thickness of the mixture layer is 80 μm or more. 15 . The negative electrode according to claim 11 , comprising a mixed active material of at least two kinds of a graphite-based material and a silicon-containing material. 16 . A secondary battery comprising the negative electrode according to claim 11 .
17. A method for producing a negative electrode binder composition according to any one of claims 1 to 10, comprising: a step of thickening an aqueous slurry consisting of at least an active material and the water-soluble resin (X); and a subsequent step of reducing the solid content concentration and mixing the aqueous latex resin (Y).