Dry-wet conversion nanofiber dressing and preparation method thereof

The dry-wet-convertible nanofiber dressing prepared by hand-held electrospinning equipment solves the problem that traditional dressings are difficult to maintain dry-wet-balance in humid environments, realizes the adaptability and safety of the wound healing environment, and avoids the risk of cytotoxicity.

CN119074984APending Publication Date: 2024-12-06SHAOXING UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410837047.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Traditional dressings are difficult to adapt to different wound types, especially in humid environments, which leads to the impact of wound infection and healing. The organic solvents used at the same time are cytotoxic, limiting their application.

Method used

Hand-held electrospinning equipment is used to prepare dry-wet-convertible nanofiber dressings. By dissolving polyvinyl alcohol, silk fibroin, sodium alginate and gelatin methacrylic acid in water, stirring and heating to form a spinning liquid, and irradiating with ultraviolet light It has dry and wet conversion characteristics and avoids the use of organic solvents.

Benefits of technology

It realizes the adjustment of the humidity level according to the amount of wound exudate, creates a suitable healing environment, avoids bacterial growth, improves wound healing efficiency and reduces the risk of cytotoxicity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119074984A_ABST
    Figure CN119074984A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps: S1, dissolving polyvinyl alcohol, silk fibroin, sodium alginate and methacrylic acid gelatin in water, stirring and heating to obtain a spinning solution; s2, electrospinning the spinning solution in the step S1 into a nanofiber membrane through handheld electrospinning equipment; and S3, irradiating the nanofiber membrane obtained in the S2 with an ultraviolet lamp to obtain the nanofiber dressing capable of being subjected to dry-wet conversion. According to the nanofiber dressing capable of being converted between the dry state and the wet state, the wet degree of the dressing can be adjusted according to the amount of wound exudate through the dry-wet conversion characteristic, a suitable healing environment is created for a wound, effective utilization of the exudate is achieved, and the purpose of exudate nourishing is achieved; the water-phase nanofiber dressing constructed by the nanofiber dressing capable of being subjected to dry-wet conversion disclosed by the invention avoids the use of an organic solvent, so that the potential cytotoxicity is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of medical dressings, and in particular to a nanofiber dressing capable of dry-wet conversion and a preparation method thereof. Background Art

[0002] The increasing frequency of fires and the rise of outdoor sports have greatly increased the frequency of skin trauma. Skin trauma has irregular shapes and varying depths. Traditional dressings are difficult to achieve emergency treatment and cannot meet the needs of different wounds for a healing environment.

[0003] The handheld electrospinning device is lightweight and portable. It can prepare nanofiber membranes with large specific surface area, high porosity and flexibility. It can deposit biofunctional materials in situ on the affected area to achieve timely and effective treatment of the wound surface. Compared with industrially produced finished dressings, the on-site operability of the portable electrospinning device makes the prepared dressings more flexible in terms of physical form: the thickness and shape of the dressing can be effectively controlled according to the location and severity of the wound; the residual trace charge on the dressing can achieve natural adhesion between the membrane and the wound surface, which can effectively prevent bacteria and microorganisms from contacting the wound from the edge of the dressing, showing great application potential in the emergency treatment of acute wounds.

[0004] Moist wounds are conducive to wound healing. However, moist conditions are prone to breed bacteria, leading to wound infection. An overly moist environment leads to maceration, edema and infection of the wound edge, which in turn causes functional damage to the skin around the wound, thus affecting wound healing. Therefore, it is necessary to create a wound healing environment according to the wound condition and maintain a dry-wet balance at the wound site for wound healing. For dry wounds with less wound exudate, keeping the wound surface slightly moist and preventing external microbial invasion can help wound healing. For moist wounds with more exudate, removing wound exudate while maintaining a moist wound environment is beneficial to wound healing. However, the currently prepared in situ deposited nanofiber dressings are difficult to adapt to a variety of wound types, limiting their application in wound healing.

[0005] At the same time, the spinning solution currently used for in-situ deposition inevitably uses organic solvents and other solvents with certain irritation. The incomplete volatilization of these solvents will make the constructed dressings potentially cytotoxic, which is not conducive to wound recovery. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a nanofiber dressing that can be converted from dry to wet and is suitable for wounds with various exudation degrees, and a preparation method thereof.

[0007] The first object of the present invention is to provide a method for preparing a nanofiber dressing that can be converted from dry to wet, comprising the following steps:

[0008] S1, dissolving polyvinyl alcohol, silk fibroin, sodium alginate and methacrylate gelatin in water, stirring and heating to obtain a spinning solution;

[0009] S2, electrospinning the spinning solution described in S1 into a nanofiber membrane by a handheld electrospinning device;

[0010] S3. Irradiate the nanofiber membrane described in S2 with ultraviolet light to obtain the nanofiber dressing capable of dry-wet conversion.

[0011] Furthermore, in S1, the mass concentration of polyvinyl alcohol in the spinning solution is 10%, the mass concentration of silk fibroin is 1%-8%, the mass concentration of sodium alginate is 1.5%-4.0%, and the mass concentration of methacrylate gelatin is 1%-5%.

[0012] Furthermore, in S1, the polyvinyl alcohol is 1788 type, and the alcoholysis degree is 87.0-89.0%.

[0013] Furthermore, in S1, the spinning solution also includes antibacterial and anti-inflammatory drugs.

[0014] Furthermore, the antibacterial and anti-inflammatory drug is selected from any one of minocycline, doxycycline, diclofenac, enoxacin, ciprofloxacin, metronidazole, clarithromycin, and azithromycin.

[0015] Furthermore, in S1, the stirring and heating temperature is 60°C-65°C.

[0016] Further, in S2, the nanofiber membrane is prepared by in-situ deposition using a handheld electrospinning device and has an irregular shape. It absorbs exudate and reaches stability, and the amount of liquid absorbed can reach 4-8 times of its own weight by adjusting the content of SA.

[0017] Furthermore, in S3, the ultraviolet light irradiation time is 5s-16s, so that the methacrylated gelatin is cross-linked, thereby enhancing the mechanical properties of the nanofiber dressing.

[0018] The second object of the present invention is to provide a nanofiber dressing that can be converted between dry and wet and is prepared by the method described above.

[0019] Furthermore, the average pore size of the dry-wet convertible nanofiber dressing is 1.31 μm-2.98 μm, and the fiber size is 250 nm-1050 nm.

[0020] Furthermore, the dry-wet convertible nanofiber dressing can be used in daily care of acute wounds, emergency treatments and chronic wounds in different situations.

[0021] Furthermore, the different occasions refer to outdoor sports venues, home and other private places, hospitals and other medical institutions; it is suitable for daily operations in outdoor venues and daily medical reserves in the home to achieve emergency treatment of sudden wounds, so as to provide timely and effective protection for acute wounds; it is suitable for daily operations in hospitals, and can provide effective protection for common wounds, and can absorb moisture to promote healing, reduce scars and the like.

[0022] Furthermore, the acute wound refers to a wound caused by sudden accidents such as falls, abrasions, falls, burns, etc.

[0023] Furthermore, the chronic wound refers to skin trauma caused by diabetes, bedsores caused by long-term bed rest, etc.

[0024] The principle of the present invention is as follows:

[0025] The constructed wound dressing, sodium alginate can absorb wound exudate, making the dressing undergo a "dry-wet" conversion, creating a healing environment with suitable humidity for wounds of different depths, preventing fluid accumulation on the wound surface, and effectively utilizing wound exudate to achieve "exudate nourishment". By adjusting the content of SA, the amount of liquid absorbed can reach 4-8 times its own weight.

[0026] In addition, the materials in the system have good biocompatibility and healing properties, and can effectively promote wound healing.

[0027] The technical solution of the present invention has the following advantages over the prior art:

[0028] (1) The "dry-wet" conversion property enables the dressing to adjust its own moisture level according to the amount of wound exudate, creating a suitable healing environment for the wound, making effective use of the exudate, and achieving the purpose of "exudate nourishment". On the one hand, for deep wounds with more exudate, no fluid accumulation is achieved; on the other hand, for shallow wounds with less exudate, "exudate nourishment" can be achieved.

[0029] (2) The aqueous nanofiber dressing constructed by the dry-wet convertible nanofiber dressing of the present invention has good air permeability and avoids the use of organic solvents, thereby avoiding potential cytotoxicity.

[0030] (3) The dry-wet convertible nanofiber dressing of the present invention is prepared by in-situ deposition using a handheld electrospinning device. The nanofiber dressing can be freely prepared into wound dressings of suitable size and shape according to the shape of the wound. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 A comparison of the pore size distribution of the nanofiber dressings prepared in Examples 2-6 of the present invention Figure 2 Schematic diagram of the air permeability change curve of the nanofiber dressing prepared in Examples 2-6 of the present invention;

[0032] Figure 3 A comparison diagram of contact angles of nanofiber dressings prepared in Examples 2-6 of the present invention;

[0033] Figure 4 is a schematic diagram of the contact angle variation curve of the nanofiber dressing prepared in Examples 2-6 of the present invention;

[0034] Figure 5 A comparison diagram of a real photograph, a structural schematic diagram and a SEM image of the nanofiber dressing prepared in Example 2 of the present invention under dry and wet wound conditions;

[0035] Figure 6 This is a comparison of SEM images of the nanofiber dressings prepared in Examples 2-6 of the present invention after swelling;

[0036] Figure 7 is a schematic diagram of the swelling curve of the nanofiber dressing prepared in Examples 2-6 of the present invention;

[0037] Figure 8 Schematic diagram of stress / strain curves of the nanofiber dressings prepared in Examples 2-6 of the present invention and Comparative Example 1;

[0038] Fig. 9 This is a SEM image of the nanofiber dressing prepared in Example 2 of the present invention;

[0039] Fig.10 This is a SEM image of the nanofiber dressing prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0040] The present invention will be further described in detail below in conjunction with the accompanying drawings and with reference to data. It should be understood that the embodiments are only for illustrating the present invention and are not intended to limit the scope of the invention in any way.

[0041] In the present invention, unless otherwise specified, the PVA used in the examples is purchased from Sinopharm Group, model 1788.

[0042] Example 1

[0043] The method for preparing the dry-wet convertible nanofiber dressing of the present invention specifically comprises the following steps:

[0044] S1. Dissolve 10g PVA (polyvinyl alcohol) and 10g SF (silk fibroin) in 100mL water respectively, prepare PVA solution and SF solution with a concentration of 10wt% by magnetic stirring at 60°C, and mix the two solutions to prepare a PVA / SF solution with a ratio of 10:7. Secondly, add a certain amount of SA (sodium alginate) to 100mL PVA / SF solution water, and stir to prepare a uniform SA solution. Add the SA solution to the PVA / SF solution, and stir to prepare a PVA / SF / SA mixed solution. The polyvinyl alcohol is 1788 type, and the degree of alcoholysis is 87.0-89.0%.

[0045] A PVA / SF / SA / GelMA spinning solution with a PVA (polyvinyl alcohol) mass concentration of 10%, a SF (silk fibroin) mass concentration of 1%-8%, a SA (sodium alginate) mass concentration of 1.5%-4.0%, and a GelMA (gelatin methacrylate) mass concentration of 1%-5% was prepared by adding 10wt% GelMA (gelatin methacrylate) to the PVA / SF / SA mixture solution after stirring and ultrasonic treatment at a stirring temperature of 60°C-65°C.

[0046] S2. The prepared solution is deposited in situ by a portable handheld electrospinning machine to form a PVA / SF / SA / GelMA nanofiber membrane.

[0047] S3. Irradiate with ultraviolet light for 5s-16s to fully crosslink GelMA under the action of photoinitiator, so as to obtain dry-wet convertible nanofiber dressings prepared with spinning solutions of different SA concentrations.

[0048] Example 2

[0049] Different from Example 1, in step S1, in the prepared PVA / SF / SA / GelMA spinning solution, the mass concentration of PVA (polyvinyl alcohol) is 10%, the mass concentration of SF (silk fibroin) is 7%, the mass concentration of SA (sodium alginate) is 4.0%, and the mass concentration of GelMA (gelatin methacrylate) is 4%.

[0050] In step S3, irradiate with UV light for 15 seconds.

[0051] Example 3

[0052] Different from Example 2, the mass concentration of SA (sodium alginate) in the prepared PVA / SF / SA / GelMA spinning solution is 3.0%.

[0053] Example 4

[0054] Different from Example 2, the mass concentration of SA (sodium alginate) in the prepared PVA / SF / SA / GelMA spinning solution is 2.5%.

[0055] Example 5

[0056] Different from Example 2, the mass concentration of SA (sodium alginate) in the prepared PVA / SF / SA / GelMA spinning solution is 2.0%.

[0057] Example 6

[0058] Different from Example 2, the mass concentration of SA (sodium alginate) in the prepared PVA / SF / SA / GelMA spinning solution is 1.5%.

[0059] Comparative Example 1 (without addition of GelMA solution)

[0060] Different from Example 2, in step S1, GelMA (gelatin methacrylate) is not added to the spinning solution.

[0061] Comparative Example 2

[0062] Different from Example 2, in step 1, the mass concentration of SA (sodium alginate) in the prepared PVA / SF / SA / GelMA spinning solution is 5%.

[0063] Porous structure test

[0064] Based on the capillary flow porosimetry method, the porous structure of the samples, including pore size and distribution, was analyzed using a 3G zh porosimeter (Quantachrome Instruments, Florida, USA). A 5 cm × 5 cm sample (weight W0) was immersed in a simulated body fluid (SBF) at 37 °C for 0.5, 1, 2, 4, 6, 8, 12, and 24 h. Then, the sample was swollen and the residual solution was removed and weighed (W1). The swelling degree (g / g) was calculated as (W1–W0) / W0. The pore size distribution of the nanofiber dressings prepared in Examples 2-6 was compared as shown in Figure 2. Figure 1 .

[0065] The air permeability of the samples was tested on a TG461E / Ⅱ digital permeameter (Fangyuan Instruments, Wenzhou, China). The test pressure difference was set to 100Pa / mm H2O. Five valid data were measured for each sample and the average value was taken. The air permeability test results of the nanofiber dressings prepared in Examples 2-6 are shown in Figure 2. Figure 2 .

[0066] like Figure 1 As shown in Figure 2, with the decrease of SA content, the average pore size (P a) gradually decreased from 2.54μm to 1.31μm. The pore size distribution range also changed significantly. The pore size distribution of the nanofiber dressing with an SA concentration of 4.0wt% is in the range of 1.2μm-4.8μm. From its morphological structure, it can be seen that the presence of the polymer aggregate structure destroys the connecting pores formed by the accumulation of nanofibers, resulting in a larger pore size gap. At the same time, due to the less stacking of nanofibers, the pore size becomes larger. With the decrease of SA content, the spinning stability increases, the morphology of the formed nanofibers tends to be stable, the arrangement of nanofibers tends to be uniform, the pore size distribution range gradually narrows, the stacking density of nanofibers increases, and the pore size becomes smaller.

[0067] like Figure 2 As shown in the figure, for the nanofiber dressing with SA concentration of 4.0wt%, the presence of polymer agglomerate structure destroyed the gas exchange channel, but the macropores gave it good air permeability. The nanofiber dressing prepared with 3.0wt% SA had less agglomerate structure and higher pore size, which improved its air permeability. With the increase of nanofiber bulk density, the decrease of pore size, and the decrease of direct pore size, the air permeability of the nanofiber dressing gradually decreased.

[0068] Moisture absorption performance test

[0069] The contact angle of the sample was measured using a contact angle tester (OCA15EC, Data Physics Instruments, Germany) to characterize the hydrophilicity of the sample. The water contact angle of the nanofiber dressing was studied to evaluate the absorption performance of wound exudate during wound healing. The contact angle comparison results of the nanofiber dressings prepared in Examples 2-6 are shown in FIG. Figure 3 The contact angle variation curves of the nanofiber dressings prepared in Examples 2-6 are shown in FIG. Figure 4 .

[0070] from Figure 3 and Figure 4 It can be seen that for hydrophilic materials, the contact angle decreases as the solution absorption increases. As the surface roughness increases, the hydrophilicity of the material surface increases. For the nanofiber dressings prepared in Examples 2-6, as the SA concentration decreases, the contact angle decreases from 31.96° to 27.51°, indicating that the nanofiber dressings prepared with a spinning solution with a higher SA concentration have better hydrophilicity. This is mainly due to the excellent hydrophilicity of SA and the rougher surface structure of the nanofiber dressings prepared with a spinning solution with a higher SA concentration. The difference in the contact angle of the nanofiber dressing decreases as the difference in SA concentration decreases, and the stability of the surface structure of the prepared nanofiber dressing increases.

[0071] Wet-dry conversion test

[0072] The samples made of 4wt% SA solution with a size of 1cm×1cm were immersed in a small amount and a large amount of SBF (simulated body fluid) respectively. A small amount of SBF could wet the sample surface, and a large amount of SBF could completely immerse the sample. After 24h, the swollen samples were taken out and freeze-dried. The surface morphology and structure of the swollen nanofiber dressing were observed by SEM. The results are as follows Figure 5 shown.

[0073] from Figure 5 It can be seen that on the dry wound surface, the nanofiber dressing has a low degree of ion exchange and gelation; the dressing maintains its original 3D fiber structure in the absence of a hydrogel structure, providing physical protection against external contamination of the wound and absorbing a small amount of exudate.

[0074] For the moist wound surface, a large amount of ion exchange forms a hydrogel, which quickly transfers excess wound exudate and stores it in the hydrogel structure, providing moist healing conditions, while achieving effective utilization of the exudate and preventing the exudate from leaching out and causing wound infection.

[0075] At the same time, other polymer components do not gel and swell. Ungelled nanofibers are used as reinforcing materials and combined with hydrogel to form a hydrogel-nanofiber composite structure, which has strong mechanical properties and provides the necessary mechanical and structural support for the hydrogel-nanofiber composite structure. The "dry-wet" conversion characteristics and the formed hydrogel-nanofiber composite structure give the nanofiber dressing good liquid absorption performance, overcoming the disadvantage that the structure of the water-phase dressing is easily damaged after swelling.

[0076] Swelling performance test

[0077] Samples with a size of 1 cm×1 cm were immersed in a large amount of SBF. After 24 hours, the swollen samples were taken out and freeze-dried. The surface morphology and structure of the swollen nanofiber dressings were observed using SEM to study the changes in the dressing structure and morphology deposited in dry and wet wounds. The SEM image comparison of the nanofiber dressings prepared in Examples 2-6 after swelling is shown in Figure 2. Figure 6 The swelling curves of the nanofiber dressings prepared in Examples 2-6 are as follows: Figure 7 shown.

[0078] from Figure 6 and 7 It can be seen that the nanofiber dressing absorbs SBF and swells rapidly, reaching the maximum swelling degree in a short time and remaining stable. All prepared nanofiber dressings absorbed a large amount of wound exudate, and their swelling rate (Swelling degree) was 5-9 times their own weight. The liquid absorbed by the swelling can be divided into liquid absorbed by the nanofiber part, liquid absorbed by the hydrogel part, and liquid stored in the pores of the nanofibers. With the increase of SA concentration, the swelling rate gradually increased.

[0079] Tensile mechanical properties test

[0080] The stress / strain results of the nanofiber dressings prepared in Examples 2-6 and Comparative Example 1 were obtained by using an electromechanical universal testing machine (WDW-20, Shanghai Hualong Testing Instrument Co., Ltd., Shanghai, China); the gauge length was 10 cm, and the tensile speed was 50 mm / min. Figure 8 As a temporary substitute for healthy skin, wound dressings should have similar mechanical properties to healthy skin: tensile stress: 1MPa-20MPa; tensile strain: 30%-70%. Strain / stress results of nanofiber dressings are shown.

[0081] from Figure 8 It can be seen that compared with the strain / stress curve of the nanofiber dressing prepared without adding GelMA solution in Comparative Example 1 (SA: 2.5wt%), the tensile stress of the nanofiber dressing prepared by the PVA / SF / SA / GelMA solution of Examples 2-6 increased by an average of 35%, and the tensile strain increased by 32%, indicating that the photo-crosslinked network of GelMA significantly improved the mechanical properties of the prepared nanofiber dressing. These curves show that the tensile stress of all samples is in the range of 6MPa-10MPa, and the tensile strain range is 60%-70%, which are all within the required range. Therefore, the nanofiber dressing meets the mechanical performance requirements and has excellent biomechanical compliance.

[0082] Electrospinning molding performance test

[0083] like Fig. 9 and Fig.10 As shown, in Example 2, when SA is 4wt%, the electrospinning is good. In Comparative Example 2, when SA is 5wt%, during the electrospinning process, beaded structures and polymer material agglomeration occurred, and the electrospinning could not be formed.

[0084] This is because as the SA mass concentration increases, the viscosity of the spinning solution increases. When the spinning solution concentration exceeds the threshold viscosity, it cannot form fibers under the action of the electric field.

[0085] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for preparing a nanofiber dressing that can be converted from dry to wet, characterized in that: The following steps are included: S1, dissolving polyvinyl alcohol, silk fibroin, sodium alginate and methacrylate gelatin in water, stirring and heating to obtain a spinning solution; S2, electrospinning the spinning solution described in S1 into a nanofiber membrane by a handheld electrospinning device; S3. Irradiate the nanofiber membrane described in S2 with ultraviolet light to obtain the nanofiber dressing capable of dry-wet conversion.

2. The method for preparing the dry-wet convertible nanofiber dressing according to claim 1, characterized in that: In S1, the mass concentration of polyvinyl alcohol in the spinning solution is 10%, the mass concentration of silk fibroin is 1%-8%, the mass concentration of sodium alginate is 1.5%-4.0%, and the mass concentration of methacrylate gelatin is 1%-5%.

3. The method for preparing the dry-wet convertible nanofiber dressing according to claim 1, characterized in that: In S1, the polyvinyl alcohol is 1788 type, and the alcoholysis degree is 87.0-89.0%.

4. The method for preparing the dry-wet convertible nanofiber dressing according to claim 1, characterized in that: In S1, the spinning solution also includes antibacterial and anti-inflammatory drugs.

5. The method for preparing the dry-wet convertible nanofiber dressing according to claim 4, characterized in that: The antibacterial and anti-inflammatory drug is selected from any one of minocycline, doxycycline, diclofenac, enoxacin, ciprofloxacin, metronidazole, clarithromycin and azithromycin.

6. The method for preparing the dry-wet convertible nanofiber dressing according to claim 1, characterized in that: In S1, the stirring and heating temperature is 60°C-65°C.

7. The method for preparing the dry-wet convertible nanofiber dressing according to claim 1, characterized in that: In S2, the nanofiber membrane is prepared by in-situ deposition using a handheld electrospinning device.

8. The method for preparing the dry-wet convertible nanofiber dressing according to claim 1, characterized in that: In S3, the ultraviolet light irradiation time is 5s-16s.

9. A nanofiber dressing capable of being converted from dry to wet and obtained according to the preparation method according to any one of claims 1 to 8.