Micro-nano hierarchical structure fiber-based composite patch as well as preparation method and application thereof
Through the micro-nano-classified structure fiber-based composite patch, combined with microfiber warp knitted support framework and nanofiber, the problem of low stability of existing hernia repair materials is solved, and better mechanical properties and biocompatibility are achieved, promoting Cell growth reduces surgical complications.
Patent Information
- Application Number
- CN202411186329.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
AI Technical Summary
Existing hernia repair materials such as polypropylene hernia repair mesh have complications such as adhesion, pain, erosion and infection during surgery, and the stability of alternative materials is low, resulting in unsatisfactory hernia repair.
Using micro-nano-classified structure fiber-based composite patches, including micro-fiber warp knitted support framework, nanofiber and porous matrix, the combination of natural polysaccharides and proteins forms patches with rich three-dimensional micro-nano structures, providing good mechanics Performance and biocompatibility.
It improves the mechanical strength and biocompatibility of the patch, promotes the growth of cells and tissues, reduces surgical complications, and provides a more stable hernia repair effect.
Smart Images

Figure HDA0005014351400000011 
Figure HDA0005014351400000012 
Figure HDA0005014351400000013
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of implantable medical devices, and in particular relates to a micro-nano hierarchical structure fiber-based composite patch and a preparation method and application thereof. Background Art
[0002] Hernia refers to the protrusion of abdominal organs or tissues to the body surface through weak points or defects in the abdominal wall tissue, which not only affects the patient's normal life, but can even endanger life safety in severe cases. At present, tension-free herniorrhaphy is an effective way to repair hernia clinically, which can effectively reduce postoperative pain and recurrence. As a tissue repair patch used in the abdominal cavity, it should have good mechanical properties, adjustable biodegradability, good biocompatibility, the ability to promote vascularization, and the characteristics of facilitating cell and tissue growth.
[0003] The natural extracellular matrix (ECM) is a fiber network structure composed of proteins and polysaccharides. Its microscopic morphology is composed of rich three-dimensional micro-nano structures, which can affect the morphology, proliferation and differentiation of human cells and participate in the migration of human cells. Studies have shown that human cells can respond to the morphological characteristics of micro-nano structures, and the filopodia of human cells can recognize the morphological characteristics of tens of nanometers, providing physical guidance signals for human cell migration, proliferation and differentiation, and promoting the regeneration of tissue cells and blood vessel growth. Therefore, suitable micro-nano hierarchical structure fiber-based composite patches have good application prospects in the field of abdominal wall hernia repair.
[0004] The polypropylene hernia repair mesh in the prior art is considered to be the most commonly used hernia repair patch in clinical practice due to its good physical, chemical and biological properties and low cost. However, polypropylene hernia repair mesh has many problems with surgical complications, including adhesion, pain, erosion and infection. Researchers have also proposed the use of biocompatible materials such as proteins, peptides, and hydrogels to replace polypropylene hernia repair meshes to minimize the side effects of the patch. These alternative materials have achieved certain results, but due to the low stability of these alternative materials, the effect of hernia repair is not ideal.
[0005] The Chinese patent with publication number CN101773689A provides a surgical repair patch, which uses electrostatic spinning to make a polymer material into a surgical biological patch with a thickness of 0.6 to 1.2 mm, and coats the surface of the patch with hyaluronic acid and collagen. The patch made by electrostatic spinning in this patent is thicker and cannot form a micron and nano interlaced structure. When used for surgical repair, it makes it difficult for cells and tissues to attach, migrate, proliferate and differentiate. In addition, this patent uses a spray gun to coat the film, which causes hyaluronic acid and collagen to be unable to penetrate the patch, resulting in uneven patch coating, which damages the biocompatibility of the patch and the affinity of the matrix tissue.
[0006] The Chinese patent with publication number CN114699556A discloses a method for preparing a silk fibroin repair patch and a silk fibroin repair patch. The patent electrospins a silk fibroin solution to obtain a silk fibroin fiber membrane. The thickness of the silk fibroin repair patch disclosed in the patent is 0.5 to 3 mm, which is relatively thick. In addition, due to incomplete dissolution of the silk fibroin, the silk fibroin cannot penetrate the patch, resulting in uneven biocompatibility of the patch. Since only a single component of silk fibroin is used to prepare the repair patch, there is a problem of poor mechanical properties. Summary of the invention
[0007] In view of this, the purpose of the present invention is to provide a micro-nano hierarchical structure fiber-based composite patch and its preparation method and application. The micro-nano hierarchical structure fiber-based composite patch provided by the present invention has good mechanical properties, biodegradability, good biocompatibility and is conducive to tissue and cell growth.
[0008] To solve the above problems, the specific implementation scheme of the present invention is as follows:
[0009] The present invention provides a micro-nano hierarchical structure fiber-based composite patch, comprising a micron fiber warp knitting support skeleton, nanofibers and a porous matrix;
[0010] The micron fiber warp knitted support skeleton is a warp knitted mesh; the nanofibers are attached to both sides of the warp knitted mesh and are interspersed in the pores of the warp knitted mesh; the porous matrix is wrapped on the warp knitted mesh and the nanofibers, and is filled in the pores of the warp knitted mesh and the nanofibers; the porous matrix includes natural polysaccharides and proteins.
[0011] Preferably, the mass proportion of the micron fiber warp knitted support skeleton is 80-95%, the mass proportion of the nanofiber is 2-8%, and the porous matrix is 3-12%;
[0012] The micron hierarchical structure pores of the micro-nano hierarchical structure fiber-based composite patch are 50 to 500 μm; the nanometer hierarchical structure pores of the micro-nano hierarchical structure fiber-based composite patch are 50 to 500 nm; the total porosity of the micro-nano hierarchical structure fiber-based composite patch is 40 to 90%; the total thickness of the micro-nano hierarchical structure fiber-based composite patch is 150 to 450 μm.
[0013] Preferably, the warp knitted mesh is woven from a substrate; the substrate includes one or more of polypropylene monofilaments, polytetrafluoroethylene monofilaments, polyglycolic acid monofilaments, polylactic acid monofilaments, polycaprolactone monofilaments and silk fibroin fibers; the diameter of the substrate is 20 to 150 μm.
[0014] Preferably, the nanofibers are cellulose nanofibers and / or silk nanofibers;
[0015] The natural polysaccharide is one or more of alginate, chitosan and hyaluronic acid;
[0016] The protein is one or more of collagen, silk fibroin and gelatin.
[0017] Preferably, the warp knitted mesh has a thickness of 100-300 μm, a pore size of 200-500 μm, and a surface density of 20-90 g / m 2 ;
[0018] The diameter of the nanofiber is 40-500 nm, and the surface density is 5-20 g / m 2 ;
[0019] The surface density of the porous matrix is 2 to 20 g / cm 2 , the pore size of the porous matrix is 50 to 300 μm.
[0020] Preferably, the warp tensile breaking strength of the micro-nano hierarchical structure fiber-based composite patch is 40-100 N / cm, the warp tensile breaking elongation is 20-70%, and the warp initial modulus is 0-1.5 kPa, and is not 0; under the condition of a fixed elongation of 20%, after cyclic stretching for 100 times, the retention rate of the warp tensile breaking strength of the micro-nano hierarchical structure fiber-based composite patch is ≥90%;
[0021] The micro-nano hierarchical structure fiber-based composite patch has a weft tensile breaking strength of 40 to 100 N / cm, a weft tensile breaking elongation of 20 to 70%, and a weft initial modulus of 0 to 1.5 kPa, and is not 0; under the condition of a fixed elongation of 20%, after cyclic stretching for 100 times, the retention rate of the weft tensile breaking strength of the micro-nano hierarchical structure fiber-based composite patch is ≥90%.
[0022] The present invention also provides a method for preparing the micro-nano hierarchical structure fiber-based composite patch described in the above technical solution, comprising the following steps:
[0023] Provide natural polysaccharide and protein mixed solution;
[0024] Adding nanofibers to the natural polysaccharide and protein mixed solution to obtain a nanofiber precursor solution;
[0025] The warp knitted mesh is added into the nanofiber precursor solution, and after being rolled, a post-treatment is performed to obtain the micro-nano hierarchical structure fiber-based composite patch.
[0026] Preferably, the mass ratio of natural polysaccharide to protein in the natural polysaccharide and protein mixed solution is 1 to 5:1; the mass concentration of natural polysaccharide in the natural polysaccharide and protein mixed solution is 2 to 12%;
[0027] The mass ratio of the warp knitted mesh, protein and nanofiber is 40-90:2-8:1.
[0028] Preferably, the post-treatment comprises one of immersion or steam treatment; the medium used for the immersion or steam treatment is independently one or more of 75wt% ethanol solution, 75wt% methanol solution, 0.5wt% glutaraldehyde aqueous solution and 0.5wt% glutaraldehyde anhydrous ethanol solution.
[0029] The present invention also provides the use of the micro-nano hierarchical structure fiber-based composite patch described in the above technical solution or the micro-nano hierarchical structure fiber-based composite patch prepared by the preparation method in the preparation of composite hernia repair products.
[0030] The present invention provides a micro-nano hierarchical fiber-based composite patch, comprising a micron fiber warp knitting support skeleton, nanofibers and a porous matrix; the micron fiber warp knitting support skeleton is a warp knitted mesh; the nanofibers are attached to both sides of the textile warp knitted mesh and are interspersed in the pores of the warp knitted mesh; the porous matrix is wrapped on the warp knitted mesh and the nanofibers, and is filled in the pores of the warp knitted mesh and the nanofibers; the porous matrix comprises natural polysaccharides and proteins.
[0031] The present invention uses a warp knitted mesh as a skeleton to ensure the mechanical strength of the micro-nano hierarchical structure fiber-based composite patch; at the same time, nanofibers made of natural raw materials are attached to both sides of the warp knitted mesh, and the nanofibers are evenly interspersed in the pores of the warp knitted mesh, and can form a rich three-dimensional micro-nano structure together with the micron fiber warp knitted supporting skeleton; the porous matrix includes natural polysaccharides and proteins, and the porous matrix with excellent biocompatibility formed by natural polysaccharides and proteins is evenly wrapped on the warp knitted mesh and nanofibers, and is evenly filled in the pores of the warp knitted mesh and nanofibers, so as to obtain the micro-nano hierarchical structure fiber-based composite patch. When used in surgical operations, the micro-nano hierarchical fiber-based composite patch provided by the present invention can provide physical guidance signals for cell migration, proliferation and differentiation, and promote the attachment and growth of tissue cells by virtue of its rich three-dimensional micro-nano structure; it also has sufficient mechanical strength to provide reliable attachment and bearing for the growth and proliferation of human cells; at the same time, the nanofibers and porous matrix have good biocompatibility and affinity for body tissues, and can promote the growth of peritoneal mesenchymal cells and the formation of new mesenchymal cell layers. Therefore, the micro-nano hierarchical fiber-based composite patch provided by the present invention has better stability, can also provide matching mechanical support, has a simple preparation process, is safe and non-toxic, and has good application prospects in the field of abdominal wall hernia repair.
[0032] The results of the embodiments show that the tensile breaking strength of the micro-nano hierarchical structure fiber-based composite patch provided by the present invention in the warp and weft directions is 40-100 N / cm, the tensile breaking elongation in the warp and weft directions is 20-70%, and the initial modulus in the warp and weft directions is 0-1.5 kPa, and is not 0; under the condition of a fixed elongation of 20%, after cyclic stretching for 100 times, the retention rate of the tensile breaking strength in the warp and weft directions of the micro-nano hierarchical structure fiber-based composite patch is ≥90%, has good mechanical properties, and can be used for abdominal hernia repair surgery.
[0033] The present invention also provides a method for preparing the micro-nano hierarchical structure fiber-based composite patch, comprising the following steps: providing a mixed solution of natural polysaccharides and proteins; adding nanofibers to the mixed solution of natural polysaccharides and proteins to mix and obtain a nanofiber precursor solution; adding a warp knitted mesh to the nanofiber precursor solution, and performing post-treatment after impregnation to obtain the micro-nano hierarchical structure fiber-based composite patch. The present invention uses a warp knitted mesh as a supporting skeleton to provide mechanical performance support for the micro-nano hierarchical structure fiber-based composite patch; the present invention mixes the nanofibers with a mixed solution of natural polysaccharides and proteins evenly, and through padding, the nanofibers are evenly attached to both sides of the warp knitted mesh and interspersed in the pores of the warp knitted mesh, and can form a rich three-dimensional micro-nano structure with the micron fiber warp knitting supporting skeleton; and after padding, the porous matrix formed by natural polysaccharides and proteins is evenly wrapped on the warp knitted mesh and the nanofibers, and filled in the pores of the warp knitted mesh and the nanofibers, so that the micro-nano hierarchical structure fiber-based composite patch has good biocompatibility and body tissue affinity, and can promote the growth of peritoneal mesenchymal cells and the formation of new mesenchymal cell layers. The preparation method provided by the present invention has a simple and controllable preparation process, a wide source of raw materials, low cost, and has industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a SEM image of the silk nanofibers prepared in Example 1;
[0035] Figure 2 This is a SEM image of the micro-nano hierarchical structure fiber-based composite patch prepared in Example 1;
[0036] Figure 3 This is a cell staining image of the micro-nano hierarchical structure fiber-based composite patch prepared in Example 1;
[0037] Figure 4 This is a SEM image of the silk fibroin warp knitted mesh prepared in Comparative Example 1;
[0038] Figure 5 This is a cell staining image of the silk fibroin warp knitted mesh prepared in Comparative Example 1. DETAILED DESCRIPTION
[0039] The present invention provides a micro-nano hierarchical structure fiber-based composite patch, comprising a micron fiber warp knitting support skeleton, nanofibers and a porous matrix;
[0040] The micron fiber warp knitted support skeleton is a warp knitted mesh; the nanofibers are attached to both sides of the warp knitted mesh and are interspersed in the pores of the warp knitted mesh; the porous matrix is wrapped on the warp knitted mesh and the nanofibers, and is filled in the pores of the warp knitted mesh and the nanofibers; the porous matrix includes natural polysaccharides and proteins.
[0041] In the present invention, unless otherwise specified, the raw materials used in the present invention are preferably commercially available products.
[0042] In the present invention, the micron hierarchical structure pores of the micro-nano hierarchical structure fiber-based composite patch are preferably 50-500 μm, more preferably 100-350 μm. In the present invention, the nanometer hierarchical structure pores of the micro-nano hierarchical structure fiber-based composite patch are preferably 50-500 nm, more preferably 50-150 nm. In the present invention, the total porosity of the micro-nano hierarchical structure fiber-based composite patch is preferably 40-90%, more preferably 65-80%. In the present invention, the total thickness of the micro-nano hierarchical structure fiber-based composite patch is preferably 150-450 μm, more preferably 150-350 μm.
[0043] The micro-nano hierarchical structure fiber-based composite patch provided by the present invention includes a micron fiber warp knitted support skeleton, and the mass proportion of the micron fiber warp knitted support skeleton in the micro-nano hierarchical structure fiber-based composite patch is preferably 80-95%. In the present invention, the micron fiber warp knitted support skeleton is a warp knitted mesh. In the present invention, the thickness of the warp knitted mesh is preferably 100-300μm, more preferably 100-250μm. In the present invention, the pore size of the warp knitted mesh is preferably 200-500μm, more preferably 200-350μm. In the present invention, the surface density of the warp knitted mesh is preferably 20-90g / m 2 , more preferably 30 to 60 g / m 2 .
[0044] In the present invention, the warp knitted mesh is preferably woven from a base material. In the present invention, the mesh shape of the warp knitted mesh is preferably rhombus, square, circular or hexagonal. The present invention has no specific requirements for the weaving, and the requirements of the present invention can be achieved according to conventional operations in the field.
[0045] In the present invention, the base material of the warp knitted mesh preferably includes one or more of polypropylene monofilaments, polytetrafluoroethylene monofilaments, polyglycolic acid monofilaments, polylactic acid monofilaments, polycaprolactone monofilaments and silk fibroin fibers, more preferably silk fibroin fibers and / or polypropylene monofilaments. In the present invention, the diameter of the base material is preferably 20 to 150 μm, more preferably 20 to 50 μm.
[0046] In the present invention, when the substrate is a silk protein fiber, the warp knitted mesh is preferably subjected to degumming treatment and ultrasonic cleaning in sequence, and the degumming treatment preferably includes high-pressure steam degumming or 5% (w / v) sodium carbonate solution immersion degumming, more preferably high-pressure steam degumming treatment. In the present invention, when the substrate is a polypropylene monofilament, a polytetrafluoroethylene monofilament, a polyglycolic acid monofilament, a polylactic acid monofilament or a polycaprolactone monofilament, the warp knitted mesh is preferably only subjected to ultrasonic cleaning. In the present invention, the ultrasonic cleaning preferably includes: placing the warp knitted mesh in a solvent at room temperature to 90°C for ultrasonic cleaning, the ultrasonic cleaning time is preferably 15 to 30 minutes, more preferably 20 minutes, and the power is preferably 10 to 25W, more preferably 20W. In the present invention, the solvent preferably includes one of deionized water, acetone, 75% ethanol and anhydrous ethanol. In the present invention, after the ultrasonic cleaning, the warp knitted mesh is preferably cleaned with deionized water and dried.
[0047] In the present invention, the high-pressure steam degumming preferably includes: soaking the warp-knitted mesh of silk fibroin fiber in deionized water for 20 to 50 minutes; then moving it into a high-pressure steam cooker for high-pressure steam degumming, the temperature of the high-pressure steam is preferably 120 to 150°C, more preferably 125°C; the time of the high-pressure steam degumming is preferably 50 to 90 minutes, more preferably 90 minutes. In the present invention, 5% (w / v) sodium carbonate solution soaking degumming preferably includes: soaking the warp-knitted mesh of silk fibroin fiber in sodium carbonate solution for preferably 20 to 50 minutes, and the concentration of the sodium carbonate solution is preferably 50g / L. In the present invention, ultrasonic cleaning is preferably performed after degumming.
[0048] The micro-nano hierarchical fiber-based composite patch provided by the present invention includes nanofibers, and the mass proportion of the nanofibers in the micro-nano hierarchical fiber-based composite patch is preferably 2-8%, and more preferably 3-5%. In the present invention, the diameter of the nanofibers is preferably 40-500nm, and more preferably 80-150nm. In the present invention, the surface density of the nanofibers is preferably 5-20g / m 2 , more preferably 10 to 15 g / m 2 .
[0049] In the present invention, the nanofiber is preferably cellulose nanofiber and / or silk nanofiber. The silk nanofiber is a fiber stripped from a natural polymer, has a multi-scale hierarchical structure, and has the advantages of renewability, biocompatibility, biodegradability and low cost. The cellulose nanofiber is stripped from cellulose, which is the most widely distributed and most abundant in nature, has a bionic hierarchical structure, and has the advantages of abundant and renewable sources, degradability, biocompatibility and low density.
[0050] The micro-nano hierarchical fiber-based composite patch provided by the present invention comprises a porous matrix, and the mass proportion of the porous matrix in the micro-nano hierarchical fiber-based composite patch is preferably 3-12%, more preferably 5-10%. In the present invention, the surface density of the porous matrix is preferably 2-20 g / cm 2 , more preferably 5 to 15 g / cm 2 . In the present invention, the pore size of the porous matrix is 50 to 300 μm, more preferably 150 to 300 μm. In the present invention, the porous matrix preferably includes natural polysaccharides and proteins. In the present invention, the natural polysaccharide is preferably one or more of alginate, chitosan and hyaluronic acid, more preferably chitosan, and the chitosan preferably has a deacetylation degree ≥ 95%. In the present invention, the chitosan / alginate / hyaluronic acid is a long-chain polymer formed by monosaccharides connected together by glycosidic bonds, and has the advantages of biocompatibility, biological activity, homogeneity and bioadhesion. In the present invention, the protein is preferably one or more of collagen, silk fibroin and gelatin, more preferably silk fibroin, which has a controllable porous structure and controllable biodegradability, and has the advantages of biocompatibility, excellent mechanical properties, slow degradation rate, and strong cell adhesion and proliferation ability.
[0051] The micro-nano hierarchical structure fiber-based composite patch provided by the present invention preferably has a warp tensile strength of 40 to 100 N / cm, a warp tensile elongation at break of 20 to 70%, and a warp initial modulus of 0 to 1.5 kPa, which is not 0; preferably, under the condition of a fixed elongation of 20%, after 100 cycles of stretching, the retention rate of the warp tensile strength of the micro-nano hierarchical structure fiber-based composite patch is ≥ 90%. The micro-nano hierarchical structure fiber-based composite patch provided by the present invention preferably has a weft tensile strength of 40 to 100 N / cm, a weft tensile elongation at break of 20 to 70%, and a weft initial modulus of 0 to 1.5 kPa, which is not 0; preferably, under the condition of a fixed elongation of 20%, after 100 cycles of stretching, the retention rate of the weft tensile strength of the micro-nano hierarchical structure fiber-based composite patch is ≥ 90%.
[0052] The present invention provides a method for preparing the micro-nano hierarchical structure fiber-based composite patch, comprising the following steps:
[0053] Provide natural polysaccharide and protein mixed solution;
[0054] Adding nanofibers to the natural polysaccharide and protein mixed solution to obtain a nanofiber precursor solution;
[0055] The warp knitted mesh is added into the nanofiber precursor solution, and after being rolled, a post-treatment is performed to obtain the micro-nano hierarchical structure fiber-based composite patch.
[0056] The invention provides a mixed solution of natural polysaccharide and protein.
[0057] In the present invention, the natural polysaccharide and protein mixed solution is preferably prepared under magnetic stirring conditions, the stirring time is preferably 0.5 to 8 hours, and the stirring temperature is preferably 20 to 100°C.
[0058] In the present invention, the mass ratio of natural polysaccharide to protein in the natural polysaccharide and protein mixed solution is preferably 1-5:1, more preferably 1-3:1. In the present invention, the mass concentration of natural polysaccharide in the natural polysaccharide and protein mixed solution is preferably 2-12%, more preferably 2-6%.
[0059] In the present invention, the preparation method of the natural polysaccharide solution is preferably: mixing the natural polysaccharide with a solvent to obtain the natural polysaccharide solution. In the present invention, when the natural polysaccharide is chitosan, the solvent is preferably an acetic acid solution with a mass concentration of 1%. In the present invention, when the natural polysaccharide is alginate or hyaluronic acid, the solvent is preferably deionized water or pure water. In the present invention, the amount ratio of the natural polysaccharide to the solvent is 1g:20-50mL.
[0060] In the present invention, the preparation operation of the protein solution is preferably: mixing the protein with water to obtain the protein solution. In the present invention, the water is preferably deionized water or pure water. In the present invention, when the protein is collagen or silk fibroin, the mixing is preferably stirred and mixed uniformly at room temperature. In the present invention, when the protein is gelatin, the mixing is preferably stirred and mixed uniformly under the condition of heating to 50°C. In the present invention, the concentration of the protein solution is preferably 2% by mass.
[0061] In the present invention, the method for preparing the mixed solution of natural polysaccharide and protein preferably comprises: adding natural polysaccharide to protein solution, or adding protein to natural polysaccharide solution, or mixing natural polysaccharide solution with protein solution.
[0062] After obtaining the natural polysaccharide and protein mixed solution, the present invention adds nanofibers into the natural polysaccharide and protein mixed solution to obtain a nanofiber precursor solution.
[0063] In the present invention, the nanofibers are preferably used in the form of a nanofiber solution, and the concentration of the nanofiber solution is preferably 0.5% (w / v). In the present invention, the nanofibers are formulated into a solution for better storage and subsequent use.
[0064] In the present invention, the mass ratio of the nanofiber solution to the natural polysaccharide and protein mixed solution is preferably 1:5-20, more preferably 1:5-8. In the present invention, the uniform mixing method is preferably oscillation, and the oscillation is preferably ultrasonic oscillation, the power of the ultrasonic oscillation is preferably 10-25W, and the time of ultrasonic oscillation is preferably 0.5-2h. The purpose of the preferred ultrasonic oscillation in the present invention is to enable the nanofibers to be fully dispersed in the precursor solution.
[0065] In the present invention, the method for preparing the silk nanofiber solution preferably includes: peeling off silk fibers layer by layer from natural degummed silk, dissolving the silk fibers in a treatment solution at -18°C, and then after 4 to 8 times of vigorous stirring at a speed of 500 to 1000 rpm, repeatedly centrifuging 5 to 12 times to wash and separate the silk fiber pulp; placing the silk fiber pulp in an ultrasonic pulverizer, with an ultrasonic power of 70W for 60 minutes to obtain a silk nanofiber suspension; concentrating the silk nanofiber suspension to 4% (w / v); taking an appropriate amount of the silk nanofiber suspension, adding deionized water to dilute to 0.5% (w / v), and obtaining the silk nanofiber solution. In the present invention, the treatment solution is preferably a mixture of NaOH, urea and H2O, and the ratio of NaOH, urea and water in the mixture is preferably 7g:12g:70 to 82mL.
[0066] In the present invention, the cellulose nanofiber solution is preferably prepared by TEMPO oxidation method combined with high-pressure homogenization method, and the specific operation steps preferably include: dispersing cellulose in a buffer solution to obtain the cellulose solution; adjusting the pH value of the cellulose solution to 10.2, adding 0.16g 2,2,6,6-tetramethylpiperidinyl oxide (TEMPO), 1.6g NaBr (analytical grade) and 50mL NaClO solution (10wt%) in sequence, stirring and mixing at 500rpm, placing at room temperature and protected from light, and performing oxidation reaction; during the oxidation reaction, preferably using an acidity meter to monitor the pH value, and detecting the pH value every 5min until the pH value no longer changes; adding 50mL of anhydrous ethanol to terminate the reaction to obtain a reaction solution; centrifuging the reaction solution at 6000rpm for 10min, collecting the precipitate; washing the obtained precipitate with deionized water for 5 times, and finally placing the obtained precipitate in a high-pressure homogenizer, homogenizing at 100Bar until it is transparent and free of particles to obtain the cellulose nanofibers (CNFs), and storing at 4°C. In the present invention, the buffer solution is prepared by dissolving 18.55 g of sodium carbonate and 6.3 g of sodium bicarbonate in 1 L of deionized water. In the present invention, the amount ratio of the cellulose to the buffer solution is 1 g:5 mL. In the present invention, the cellulose is preferably microcrystalline cellulose (MCC), which has the advantages of chemical stability and biological safety.
[0067] After obtaining the nanofiber precursor solution, the present invention adds the warp knitted mesh into the nanofiber precursor solution, and after impregnation and rolling, performs post-treatment to obtain the micro-nano hierarchical structure fiber-based composite patch.
[0068] In the present invention, the mass ratio of the warp knitted mesh, nanofibers and protein is 40-90:2-8:1, more preferably 60-80:2-5:1.
[0069] In the present invention, the specific operation of impregnation preferably includes: immersing the warp knitted mesh in the nanofiber precursor solution for 20 to 60 minutes, and then preferably using a scraper to apply the nanofiber precursor solution to both sides of the warp knitted mesh for 3 times to obtain an impregnated sheet.
[0070] In the present invention, the impregnation can ensure that the warp knitted mesh is fully impregnated with the nanofiber precursor solution, and the obtained impregnated sheet is placed in the post-treatment solution, which is conducive to fixing the coating on the surface of the impregnated sheet. The purpose of the scraper used in the present invention is to control the uniform coating of the mesh surface, ensure that the nanofibers are fully dispersed and coated, and ensure that the nanofibers are uniformly deposited and wrapped around the warp knitted mesh and interspersed in the pores of the warp knitted mesh; the present invention uses a small amount of repeated coating to ensure that the natural polysaccharide and protein mixed solution is fully impregnated on the micron substrate and the nanofibers, and ensure the bonding strength of the two fibers with different diameters and the stable and non-dispersed structure of the patch.
[0071] In the present invention, the post-treatment preferably comprises one of immersion or steam treatment. In the present invention, the medium used in the immersion or steam treatment is independently preferably one or more of 75wt% ethanol solution, 75wt% methanol solution, 0.5wt% glutaraldehyde aqueous solution and 0.5wt% glutaraldehyde anhydrous ethanol solution, more preferably 75wt% ethanol solution.
[0072] In the present invention, the specific operation of soaking preferably includes: placing the soaked sheet obtained after immersion and rolling in a post-treatment medium for 1 to 30 minutes; then washing away the nanofiber precursor solution and the post-treatment medium remaining on the surface of the soaked sheet with deionized water to obtain a micro-nano hierarchical structure fiber-based composite patch wet sheet.
[0073] In the present invention, the specific operation of the steam treatment preferably includes: placing the impregnated sheet obtained after immersion in a closed container with a post-treatment medium, using the volatilization of the post-treatment medium to induce the transformation of the porous matrix structure to obtain a wet sheet of a micro-nano hierarchical structure fiber-based composite patch; the steam treatment time is preferably 2 to 30 minutes.
[0074] After the post-treatment, the present invention preferably further comprises freeze drying. In the present invention, the freezing temperature of the freeze drying is preferably -16 to -20°C, and the time is preferably 6 to 12 hours; the drying temperature is preferably -35 to -50°C, and the time is preferably 12 to 48 hours.
[0075] In the present invention, the micro-nano hierarchical structure fiber-based composite patch is preferably stored in a sterile environment at 4°C.
[0076] The present invention also provides surgical supplies for repairing composite hernias prepared by using the micro-nano hierarchical structure fiber-based composite patch described in the above technical solution.
[0077] The technical solution of the present invention is further illustrated by specific implementation methods below. Those skilled in the art should understand that the embodiments described below are only part of the embodiments of the present invention, which are used to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0078] Example 1
[0079] (1) Preparation of warp knitted mesh
[0080] The silk fibroin fiber is woven into a warp knitted mesh with a diamond mesh shape as a micron fiber warp knitted support skeleton. The silk fibroin fiber warp knitted mesh needs to be degummed, and the specific operation steps are as follows: the warp knitted mesh is placed in deionized water and soaked for 20 minutes, and then moved into a high-pressure steam cooker for high-pressure steam degumming, and the temperature of the high-pressure steam is set to 125°C, and the high-pressure steam degumming time is 60 minutes; the sample after high-pressure steam degumming is placed in 80°C deionized water and ultrasonically cleaned, and the ultrasonic cleaning time is 20 minutes and the power is 20W; the sample after ultrasonic cleaning is cleaned with deionized water and then dried to obtain a silk fibroin fiber warp knitted mesh.
[0081] (2) Preparation of chitosan solution and gelatin solution
[0082] Weigh 3 g of chitosan (deacetylation degree ≥ 95%) powder and dissolve it in 100 mL of 1 wt % acetic acid solution, stir it with a magnetic stirrer until it is completely dissolved, and filter and remove impurities to obtain a chitosan solution.
[0083] Weigh 2 g of gelatin and dissolve it in 100 mL of pure water. Heat it in a water bath to 50°C and continue stirring until it is completely dissolved to obtain a gelatin solution.
[0084] (3) Preparation of natural polysaccharide and protein mixed solution
[0085] The obtained chitosan solution and gelatin solution were stirred and mixed at a mass ratio of 1:1 for 2 h to obtain a mixed solution of chitosan and gelatin.
[0086] (4) Preparation of nanofiber solution
[0087] The silk fibers are peeled off layer by layer from the natural degummed silk, dissolved in a treatment solution at -18°C, and then subjected to 6 times of intense mechanical stirring, centrifuged repeatedly 6 times, and the silk fiber pulp is washed and separated; the obtained silk fiber pulp is placed in an ultrasonic pulverizer with an ultrasonic power of 70 W for 60 min to obtain a silk nanofiber suspension; the obtained silk nanofiber suspension is concentrated to 4% (w / v); 10 g of the obtained silk nanofiber suspension is taken, and 70 mL of deionized water is added to dilute it to 0.5 wt% (w / v) to obtain a silk nanofiber solution.
[0088] (5) Preparation of nanofiber precursor solution
[0089] The prepared silk nanofibers were mixed with a mixed solution of chitosan and gelatin at a mass ratio of 1:5, and ultrasonically oscillated at a power of 20 W for 1 h to obtain a nanofiber precursor solution.
[0090] (6) Preparation of micro-nano hierarchical fiber-based composite patches
[0091] The prepared silk fibroin fiber warp knitted mesh was immersed in the obtained nanofiber precursor solution for 30 minutes, and then fully rolled. The nanofiber precursor solution was coated on both sides of the silk fibroin fiber warp knitted mesh three times with a scraper to obtain an immersed sheet; the obtained immersed sheet was placed in a 75% ethanol solution and immersed for 1 minute; the nanofiber precursor solution and ethanol solution remaining on the surface of the immersed sheet were washed off with deionized water to obtain a wet sheet of a micro-nano hierarchical structure fiber-based composite patch; the obtained wet sheet of the micro-nano hierarchical structure fiber-based composite patch was frozen at -16°C for 12 hours, and then dried at -40°C for 48 hours to obtain a micro-nano hierarchical structure fiber-based composite patch.
[0092] According to the ISO7198 standard, the thickness of the sample is 0.5 cm. 2 In the test area, a digital display micrometer table thickness gauge was used to randomly test 10 points in the test area, and the average value was taken as the test result. The test results showed that the thickness of the silk fibroin fiber warp knitted mesh was 211 μm, and the average total thickness of the obtained micro-nano hierarchical structure fiber-based composite patch was 242 μm.
[0093] The pore size was detected by electron microscope, magnified 20 times, and at least 30 groups of pore sizes were measured on the sample, and the average value was taken as the test result. The test results showed that the pore size of the silk fibroin fiber warp knitted mesh was 300μm, the diameter of the nanofiber was 40-140nm, the pore size of the porous matrix was 150-300μm, and the micron hierarchical structure pores of the obtained micro-nano hierarchical structure fiber-based composite patch were 100-300μm, and the nano hierarchical structure pores were 50-150nm.
[0094] The porosity in the image was calculated using Photoshop image processing software using a 20-fold magnification photograph taken with an electron microscope. The calculation result was that the total porosity of the obtained micro-nano hierarchical structure fiber-based composite patch was 86%.
[0095] According to the standard ISO3801:1997, the surface density of the sample is tested. The sample is placed in a standard environment with a temperature of 25±2℃ and a humidity of 40-60% for 24 hours. The sample is cut into a 10cm×10cm square and weighed using a 1 / 10,000 precision balance. The unit area mass of the sample = the balance display result × 100, g / m 2 The test results show that the surface density of the silk fibroin fiber warp knitted mesh is 45g / m 2 The surface density of nanofibers is 12g / m 2 , the surface density of the porous matrix is 10 g / cm 2 .
[0096] According to the standard ASTM D5035-11, the tensile strength at break, elongation at break and retention of tensile strength at break of the sample were tested. It was required to cut a sample of 5cm×1.5cm in the crease-free area, and take at least 5 pieces in the longitudinal and transverse directions respectively. The test results are as follows: the tensile strength at break in the warp direction of the obtained micro-nano hierarchical structure fiber-based composite patch is 56N / cm, the initial modulus is 1.11kPa, and the elongation at break in the warp direction is 51%; the tensile strength at break in the weft direction is 51N / cm, the initial modulus is 1.50kPa, and the elongation at break in the weft direction is 62%; under the condition of a fixed elongation of 20%, after 100 cycles of stretching, the retention rate of the tensile strength at break in the warp direction is 93%, and the retention rate of the tensile strength at break in the weft direction is 90%.
[0097] Figure 1 This is the SEM image of the silk nanofibers prepared in Example 1. Figure 1 It can be seen that the diameter of silk nanofibers is distributed between 40 and 140 nm, which is consistent with the measurement results of electron microscopy and there is no significant difference.
[0098] Figure 2 This is the SEM image of the micro-nano hierarchical fiber-based composite patch prepared in Example 1. Figure 2 It can be seen that: at low magnification, a micro-nano porous structure can be seen formed on the warp knitted mesh, and at high magnification, nanoscale fibers can be seen attached to the mesh monofilaments, constructing a micro-nano hierarchical structure.
[0099] Figure 3 This is a cell staining image of the micro-nano hierarchical structure fiber-based composite patch prepared in Example 1. The living cells will show green fluorescence after being stained, and the dead cells will show red fluorescence after being stained. Figure 3It can be seen that the proportion of live cells showing green fluorescence is very high, and the distribution is uniform and extensive, indicating that all live cells are progressively proliferating, growing well, and presenting a spindle-shaped structure. And there are no dead cells with red fluorescence, indicating that there are no toxic reactions such as cell shedding, dissolution, and extensive cavitation, and no obvious dead cells are produced. Therefore, the obtained micro-nano hierarchical structure fiber-based composite patch has good cell compatibility and excellent cell adhesion promoting effect.
[0100] Example 2
[0101] The silk fibroin fiber warp knitted mesh, chitosan solution and silk nanofiber solution prepared in Example 1 were used.
[0102] (1) Preparation of natural polysaccharide and protein mixed solution
[0103] Weigh 2 g of collagen and dissolve it in 100 mL of deionized water. Stir magnetically until it is completely dissolved, and filter to remove impurities to obtain a collagen solution.
[0104] The obtained collagen solution and the chitosan solution prepared in Example 1 were stirred and mixed at a mass ratio of 1:1 for 2 hours to obtain a mixed solution of chitosan and collagen.
[0105] (2) Preparation of nanofiber precursor solution
[0106] The silk nanofiber solution prepared in Example 1 was mixed with the obtained chitosan and collagen mixed solution at a mass ratio of 1:5, and ultrasonically oscillated at a power of 20 W for 1 h to obtain a nanofiber precursor solution.
[0107] (3) Preparation of micro-nano hierarchical fiber-based composite patches
[0108] The silk fibroin fiber warp knitted mesh prepared in Example 1 was added to the prepared nanofiber precursor solution for 30 minutes, and then fully impregnated and rolled, and the nanofiber precursor solution was coated on both sides of the silk fibroin fiber warp knitted mesh three times using a scraper to obtain an impregnated sheet; the obtained impregnated sheet was immersed in a 75% ethanol solution for 60 seconds; the nanofiber precursor solution and ethanol solution remaining on the surface of the impregnated sheet were washed off with deionized water to obtain a wet sheet of a micro-nano hierarchical structure fiber-based composite patch; the obtained wet sheet of the micro-nano hierarchical structure fiber-based composite patch was frozen at -16°C for 12 hours, and then dried at -40°C for 48 hours to obtain a micro-nano hierarchical structure fiber-based composite patch.
[0109] The obtained micro-nano hierarchical fiber-based composite patch was tested, and the test results showed that the pore size of the porous matrix was 50-200 μm, the micron hierarchical structure pores of the obtained micro-nano hierarchical fiber-based composite patch were 50-150 μm, the nano hierarchical structure pores were 50-150 nm, and the total porosity was 89%. The surface density of the porous matrix was 8-15 g / cm 2 The obtained micro-nano hierarchical structure fiber-based composite patch has a warp tensile strength of 59N / cm, an initial modulus of 0.82kPa, and a warp elongation of 48%; the weft tensile strength is 53N / cm, the initial modulus is 1.36kPa, and the weft elongation is 61%; under the condition of a fixed elongation of 20%, after 100 cycles of stretching, the retention rate of the warp tensile strength at break is 92%, and the retention rate of the weft tensile strength at break is 93%.
[0110] Example 3
[0111] The silk nanofiber solution prepared in Example 1 was used.
[0112] (1) Preparation of warp knitted mesh
[0113] The polypropylene (PP) fiber is woven into a triangular mesh warp knitted mesh as a micron fiber warp knitted support skeleton. The polypropylene fiber warp knitted mesh needs to be ultrasonically cleaned, and the specific operation steps are as follows: the polypropylene fiber warp knitted mesh is placed in acetone, 75% ethanol and 100mL deionized water in turn, and ultrasonic cleaning is performed for 15 minutes in each solvent, and the ultrasonic power is 20W. After ultrasonic cleaning, it is dried to obtain a polypropylene fiber warp knitted mesh.
[0114] (2) Preparation of hyaluronic acid solution and silk fibroin solution
[0115] Weigh 2 g of hyaluronic acid and dissolve it in 100 mL of deionized water. Stir magnetically until it is completely dissolved. Filter and remove impurities to obtain a hyaluronic acid solution.
[0116] 2 g of silk fibroin was weighed and dissolved in 100 mL of deionized water. At room temperature, the solution was stirred continuously until the solution was completely dissolved to obtain a silk fibroin solution with a volume fraction of 2%.
[0117] (3) Preparation of natural polysaccharide and protein mixed solution
[0118] The obtained hyaluronic acid solution and silk fibroin solution were stirred and mixed at a mass ratio of 1:1 for 2 hours to obtain a hyaluronic acid and silk fibroin mixed solution.
[0119] (4) Preparation of nanofiber precursor solution
[0120] The silk nanofibers prepared in Example 1 were mixed with the obtained mixed solution of hyaluronic acid and silk fibroin at a mass ratio of 1:5, and ultrasonically oscillated at a power of 20 W for 1 h to obtain a nanofiber precursor solution.
[0121] (5) Preparation of micro-nano hierarchical fiber-based composite patches
[0122] The prepared polypropylene fiber warp knitted mesh was immersed in the obtained nanofiber precursor solution for 30 minutes, and then fully rolled. The nanofiber precursor solution was coated on both sides of the polypropylene fiber warp knitted mesh three times using a scraper to obtain an immersed sheet; the obtained immersed sheet was placed in a 75% ethanol solution and immersed for 60 seconds; the nanofiber precursor solution and ethanol solution remaining on the surface of the immersed sheet were washed off with deionized water to obtain a micro-nano hierarchical structure fiber-based composite patch wet sheet; the obtained micro-nano hierarchical structure fiber-based composite patch wet sheet was frozen at -16°C for 12 hours, and then dried at -40°C for 48 hours to obtain a micro-nano hierarchical structure fiber-based composite patch.
[0123] The obtained micro-nano hierarchical structure fiber-based composite patch was tested, and the test results showed that the thickness of the polypropylene fiber warp knitted mesh was 273 μm, the pore size was 350 μm, and the surface density was 68 g / m 2 ; The diameter of the nanofibers is 60-180nm, and the surface density is 8g / m 2 ; The surface density of the porous matrix is 5g / cm 2 , pore size is 250-300μm; the micron hierarchical structure pores of the obtained micro-nano hierarchical structure fiber-based composite patch are 100-300μm, the nano hierarchical structure pores are 50-150nm, and the total porosity is 90%; the warp tensile breaking strength of the obtained micro-nano hierarchical structure fiber-based composite patch is 67N / cm, the initial modulus is 1.32kPa, and the warp elongation at break is 46%; the weft tensile breaking strength is 57N / cm, the initial modulus is 1.48kPa, and the weft elongation at break is 55%; under the condition of a fixed elongation of 20%, after 100 cycles of stretching, the retention rate of the warp tensile breaking strength is 91%, and the retention rate of the weft tensile breaking strength is 90%.
[0124] Example 4
[0125] The polypropylene fiber warp knitted mesh prepared in Example 3 and the mixed solution of hyaluronic acid and silk fibroin were used.
[0126] (1) Preparation of nanofiber solution
[0127] The cellulose nanofiber solution was prepared by combining TEMPO oxidation method with high pressure homogenization method. The specific operation steps included: dissolving 18.55 g of sodium carbonate and 6.3 g of sodium bicarbonate in 1 L of deionized water to obtain a buffer solution. 10 g of cellulose was dispersed in 50 mL of the obtained buffer solution to obtain a cellulose solution; the pH value of the obtained cellulose solution was adjusted to 10.2, 0.16 g of 2,2,6,6-tetramethylpiperidinyl oxide (TEMPO), 1.6 g of NaBr (analytical grade) and 50 mL of NaClO solution (10 wt%) were added in sequence, the mixture was stirred and mixed evenly at 500 rpm, and the mixture was placed at room temperature and protected from light to perform an oxidation reaction; during the reaction, the pH value was monitored using an acidity meter, and the pH value was tested every 5 minutes until the pH value no longer changed; then 50 mL of anhydrous ethanol was added to terminate the reaction to obtain a reaction solution; the obtained reaction solution was centrifuged at 6000 rpm for 10 minutes, and the precipitate was collected; the obtained precipitate was centrifuged and washed 5 times with deionized water, and the final precipitate was placed in a high-pressure homogenizer, homogenized at 100 Bar until it was transparent and free of particles, and cellulose nanofibers (CNFs) were obtained, which were stored at 4°C. When in use, a proper amount of the obtained cellulose nanofibers is added to deionized water to prepare a concentration of 0.5% (w / v) to obtain a cellulose nanofiber solution.
[0128] (2) Preparation of nanofiber precursor solution
[0129] The prepared cellulose nanofiber solution was mixed with the mixed solution of hyaluronic acid and silk fibroin prepared in Example 3 at a mass ratio of 1:5, and ultrasonically oscillated at a power of 20 W for 2 h to obtain a nanofiber precursor solution.
[0130] (3) Preparation of micro-nano hierarchical fiber-based composite patches
[0131] The polypropylene fiber warp knitted mesh prepared in Example 3 was immersed in the obtained nanofiber precursor solution for 30 minutes, and then fully rolled. The nanofiber precursor solution was coated on both sides of the polypropylene fiber warp knitted mesh three times using a scraper to obtain an immersed sheet; the obtained immersed sheet was placed in a 75% ethanol solution and immersed for 60 seconds; the nanofiber precursor solution and ethanol solution remaining on the surface of the immersed sheet were washed off with deionized water to obtain a wet sheet of a micro-nano hierarchical structure fiber-based composite patch; the obtained wet sheet of the micro-nano hierarchical structure fiber-based composite patch was frozen at -16°C for 12 hours, and then dried at -40°C for 48 hours to obtain a micro-nano hierarchical structure fiber-based composite patch.
[0132] The obtained micro-nano hierarchical fiber-based composite patch was tested, and the test results showed that the diameter of the nanofibers was 50-200 nm, and the surface density was 8 g / m 2 The surface density of the porous matrix is 5 g / cm 2, the pore size of the porous matrix is 250-300μm. The micron hierarchical structure pores of the obtained micro-nano hierarchical structure fiber-based composite patch are 150-400μm, the nano hierarchical structure pores are 100-250nm, and the total porosity is 90%. The warp tensile strength of the obtained micro-nano hierarchical structure fiber-based composite patch is 66N / cm, the initial modulus is 0.98kPa, and the warp elongation is 47%; the weft tensile strength is 53N / cm, the initial modulus is 1.32kPa, and the weft elongation is 58%; under the condition of a fixed elongation of 20%, after 100 cycles of stretching, the retention rate of the warp tensile strength is 92%, and the retention rate of the weft tensile strength is 93%.
[0133] Comparative Example 1
[0134] The difference from Example 1 is that the warp knitted mesh with no micro-nano hierarchical structure is constructed on the surface, that is, the silk mesh made of silk fibers warp knitted in Example 1 is degummed to obtain a silk fibroin warp knitted mesh without subsequent modification.
[0135] The obtained micro-nano hierarchical structure fiber-based composite patch was tested, and the test results showed that the thickness of the silk fiber warp knitted mesh was 0.163-0.178 mm, the pore size was 182-213 μm, and the surface density was 42 g / m 2 The total porosity of the obtained micro-nano hierarchical fiber-based composite patch is 51%. The obtained micro-nano hierarchical fiber-based composite patch has a warp tensile strength of 47N / cm, an initial modulus of 1.38kPa, and a warp elongation of 54%; a weft tensile strength of 45N / cm, an initial modulus of 1.49kPa, and a weft elongation of 72%; under the condition of a fixed elongation of 20%, after 100 cycles of stretching, the retention rate of the warp tensile strength at break is 88%, and the retention rate of the weft tensile strength at break is 85%.
[0136] Figure 4 This is the SEM image of the silk fibroin warp knitted mesh prepared in Comparative Example 1. Figure 4 It can be seen that the mesh is composed of silk monofilaments with obvious mesh holes. After degumming, it is slightly deformed and the surface of the monofilaments is smooth.
[0137] Figure 5 This is a cell staining image of the silk fibroin warp knitted mesh prepared in Comparative Example 1. The living cells will show green fluorescence after being stained, and the dead cells will show red fluorescence after being stained. Figure 5 It can be seen that the active cells showing green fluorescence are scattered and small in number, indicating that only a small number of live cells adhere to the surface of the silk fibroin warp-knitted mesh, the number of cells is relatively small, and no obvious dead cells are produced.
[0138] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A micro-nano hierarchical fiber-based composite patch, characterized in that: It includes a micron fiber warp knitting support skeleton, nanofibers and a porous matrix; The micron fiber warp knitted support skeleton is a warp knitted mesh; the nanofibers are attached to both sides of the warp knitted mesh and are interspersed in the pores of the warp knitted mesh; the porous matrix is wrapped on the warp knitted mesh and the nanofibers, and is filled in the pores of the warp knitted mesh and the nanofibers; the porous matrix includes natural polysaccharides and proteins.
2. The micro-nano hierarchical structure fiber-based composite patch according to claim 1, characterized in that: The mass proportion of the micron fiber warp knitting support skeleton is 80-95%, the mass proportion of the nanofiber is 2-8%, and the porous matrix is 3-12%; The micron hierarchical structure pores of the micro-nano hierarchical structure fiber-based composite patch are 50 to 500 μm; the nanometer hierarchical structure pores of the micro-nano hierarchical structure fiber-based composite patch are 50 to 500 nm; the total porosity of the micro-nano hierarchical structure fiber-based composite patch is 40 to 90%; the total thickness of the micro-nano hierarchical structure fiber-based composite patch is 150 to 450 μm.
3. The micro-nano hierarchical structure fiber-based composite patch according to claim 1, characterized in that: The warp knitted mesh is woven from a base material; the base material comprises one or more of polypropylene monofilament, polytetrafluoroethylene monofilament, polyglycolic acid monofilament, polylactic acid monofilament, polycaprolactone monofilament and silk fibroin fiber; the diameter of the base material is 20-150 μm.
4. The micro-nano hierarchical structure fiber-based composite patch according to claim 1, characterized in that: The nanofibers are cellulose nanofibers and / or silk nanofibers; The natural polysaccharide is one or more of alginate, chitosan and hyaluronic acid; The protein is one or more of collagen, silk fibroin and gelatin.
5. The micro-nano hierarchical structure fiber-based composite patch according to claim 1, characterized in that: The warp knitted mesh has a thickness of 100 to 300 μm, a pore size of 200 to 500 μm, and a surface density of 20 to 90 g / m 2 ; The diameter of the nanofiber is 40-500 nm, and the surface density is 5-20 g / m 2 ; The surface density of the porous matrix is 2 to 20 g / cm 2 , the pore size of the porous matrix is 50 to 300 μm.
6. The micro-nano hierarchical structure fiber-based composite patch according to claim 1, characterized in that: The warp tensile breaking strength of the micro-nano hierarchical structure fiber-based composite patch is 40-100 N / cm, the warp tensile breaking elongation is 20-70%, and the warp initial modulus is 0-1.5 kPa, and is not 0; under the condition of a fixed elongation of 20%, after cyclic stretching for 100 times, the retention rate of the warp tensile breaking strength of the micro-nano hierarchical structure fiber-based composite patch is ≥90%; The micro-nano hierarchical structure fiber-based composite patch has a weft tensile breaking strength of 40 to 100 N / cm, a weft tensile breaking elongation of 20 to 70%, and a weft initial modulus of 0 to 1.5 kPa, and is not 0; under the condition of a fixed elongation of 20%, after cyclic stretching for 100 times, the retention rate of the weft tensile breaking strength of the micro-nano hierarchical structure fiber-based composite patch is ≥90%.
7. The method for preparing the micro-nano hierarchical structure fiber-based composite patch according to any one of claims 1 to 6, characterized in that: The following steps are involved: Provide natural polysaccharide and protein mixed solution; Adding nanofibers to the natural polysaccharide and protein mixed solution to obtain a nanofiber precursor solution; The warp knitted mesh is added into the nanofiber precursor solution, and after being rolled, a post-treatment is performed to obtain the micro-nano hierarchical structure fiber-based composite patch.
8. The preparation method according to claim 7, characterized in that: The mass ratio of natural polysaccharide to protein in the natural polysaccharide and protein mixed solution is 1 to 5:1; the mass concentration of natural polysaccharide in the natural polysaccharide and protein mixed solution is 2 to 12%; The mass ratio of the warp knitted mesh, protein and nanofiber is 40-90:2-8:
1.
9. The preparation method according to claim 7, characterized in that: The post-treatment includes one of soaking or steam treatment; the medium used in the soaking or steam treatment is independently one or more of 75wt% ethanol solution, 75wt% methanol solution, 0.5wt% glutaraldehyde aqueous solution and 0.5wt% glutaraldehyde anhydrous ethanol solution.
10. Use of the micro-nano hierarchical structure fiber-based composite patch according to claims 1 to 6 or the micro-nano hierarchical structure fiber-based composite patch prepared by the preparation method according to claims 7 to 9 in the preparation of composite hernia repair products.