Double non-noble metal catalyst Co-Ni / CeO2, preparation method thereof and application of double non-noble metal catalyst Co-Ni / CeO2 in catalyzing selective hydrogenation of m-xylylenediamine in heterogeneous system

Through the bis-non-noble metal catalyst Co-Ni/CeO2 without additives, the high selective hydrogenation of isophthalamine is achieved to 1,3-cyclohexylene dimethylamine, which solves the inhibition of side reactions in the prior art , high cost and stability issues have significant industrialization potential.

CN119076001APending Publication Date: 2024-12-06ANHUI UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411208183.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the existing catalytic hydrogenation technology, there are problems in which side reactions cannot be effectively suppressed, the cost of noble metal catalysts is high, and the stability needs to be improved, especially when isophthalamine selective hydrogenation is 1,3-cyclohexylene methane During the process.

Method used

The dual non-precious metal catalyst Co-Ni/CeO2 is used to support Co and Ni by sodium carbonate precipitation method, and catalyzed using an additive-free heterogeneous system. The hydrogenation rate is fast, the cost is low, and the preparation method is simple.

Benefits of technology

High selective hydrogenation catalysis has been achieved, with the conversion rate of isophthalamine of 100%, and the selectivity of 1,3-cyclohexylene amine of more than 97%, reducing the separation cost and having broad industrialization prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076001A_ABST
    Figure CN119076001A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a double non-noble metal catalyst Co-Ni / CeO2 and application of the double non-noble metal catalyst Co-Ni / CeO2 in catalyzing selective hydrogenation of m-xylylenediamine under the conditions of no additive and mild conditions in a heterogeneous system, and belongs to the field of catalytic hydrogenation. Wherein cerium oxide is used as a carrier and the total loading capacity is Co-Ni / CeO2 (wherein the ratio of Co to Ni is 1: (4-0.25)), cobalt nitrate hexahydrate is used as a cobalt source, nickel nitrate hexahydrate is used as a nickel source, cerium dioxide is used as a carrier, anhydrous sodium carbonate is used as a precipitator, active metals Co and Ni are loaded on CeO2 by using a deposition-precipitation method, the CeO2 is put into a tubular furnace and reduced by using hydrogen-argon mixed gas, and the catalyst is prepared. And passivating by using oxygen and argon mixed gas to obtain the catalyst Co-Ni / CeO2. The conversion rate reaches 100% when the catalyst is 0.1 g, the m-xylylenediamine is 0.5 g, the hydrogen pressure is 8 MPa, the temperature is 120 DEG C, and the reaction lasts for 6 h, and the selectivity of the 1, 3-cyclohexanedimethylamine reaches 97% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalytic hydrogenation, and specifically relates to a dual non-precious metal catalyst Co-Ni / CeO2 and a preparation method thereof, as well as an application of the catalyst in catalyzing the selective hydrogenation of m-xylylenediamine to 1,3-cyclohexylenediamine in a heterogeneous system. Background Art

[0002] 1,3-cyclohexylenediamine is an important organic chemical and fine chemical intermediate, which is widely used in epoxy resin, composite materials, desulfurizer, emulsifier and pesticide, etc. It is also an important raw material for synthesizing isocyanate. At present, some progress has been made in the study of the reaction catalytic system for the selective hydrogenation of m-phenylenediamine to prepare 1,3-cyclohexylenediamine, but there are still the following shortcomings: (1) It is impossible to effectively inhibit the occurrence of side reactions such as demethylation in the reaction system; (2) Precious metal catalysts are widely used in the hydrogenation of aromatic amines, but precious metals are expensive; (3) The stability of the catalyst still needs to be improved. Therefore, the development of non-precious metal-based catalysts with excellent catalytic performance is of great significance in actual industrial production and application.

[0003] At present, the most atom-economical route is to catalytically hydrogenate phenylenediamine to cyclohexanediamine, but most of the catalysts used are precious metal catalysts, such as Ru. Zhao et al. used Ru / C with a loading of 8.5wt% as a catalyst and isopropanol as a solvent. In the absence of additives, the conversion rate of o-phenylenediamine reached 99.5% at a reaction temperature of 160°C and a pressure of 7MPa, and the yield of 1,2-cyclohexanediamine reached 77.3%. Lin Xue et al. used isopropanol as a solvent and lithium hydroxide as an additive. The experimental results showed that under the conditions of 120°C and 8MPa, the conversion rate of p-phenylenediamine was 100%, the selectivity of the product 1,4-cyclohexanediamine reached 92%, and the formation of the by-product cyclohexane was effectively suppressed. Wang Tao and others from Dalian Institute of Chemical Physics used Ru / C with a loading of 5wt% as a catalyst, isopropanol as a solvent, and sodium nitrite as an additive. The conversion rate of o-phenylenediamine reached 99.5% at a reaction temperature of 170°C and a pressure of 8MPa, and the selectivity of 1,2-cyclohexanediamine reached 86.3%. After five cycles, the selectivity of the product can still reach more than 85%. Liu Qinglin and others also used the method of 500°C activation and alkali treatment of the catalyst, and found that the performance of the treated Ru / C catalyst was significantly improved. Under the conditions of 140°C and 8MPa, the conversion rate of p-phenylenediamine and the selectivity of 1,4-cyclohexanediamine were 100% and 90%, respectively.

[0004] As an important organic chemical and fine chemical intermediate, 1,3-cyclohexyl dimethylamine is widely used in the fields of desulfurizer, emulsifier and pesticide. It is also an important raw material for synthesizing isocyanate. The synthesized alicyclic isocyanate does not contain a benzene ring structure and has a relatively stable property. It can be used to prepare polyurethane products with excellent yellowing resistance. When 1,3-cyclohexyl dimethylamine is used as an alicyclic amine curing agent, it has the advantages of longer application period and lighter color than aliphatic amines. In addition, the molecular structure contains a rigid alicyclic ring, and it has excellent heat resistance, water resistance, chemical resistance and mechanical properties. However, m-phenylenediamine is a highly toxic item. Inhalation of its vapor can cause asthma and other respiratory diseases. Skin absorption leads to blood disorders and affects kidney and liver function. Therefore, it is of great research value to develop a production process for hydrogenating m-phenylenediamine to 1,3-cyclohexyl dimethylamine. For example, Yang Yanmi and others from Beijing University of Chemical Technology showed excellent catalytic effect using Ru / Al2O3 as a catalyst. Under the conditions of 5% Ru loading, 130°C reaction temperature, 5MPa reaction pressure, and tetrahydrofuran as solvent, the conversion rate of m-xylenediamine reached 100%, and the selectivity of 1,3-cyclohexylenediamine reached 87.7%. The catalyst modified by LiOH could achieve a 97.9% yield of 1,3-cyclohexylenediamine under the above conditions. Kim et al. used 5wt% Ru / C as catalyst, isopropanol as solvent, sodium nitrate as additive, and the conversion rate of m-xylenediamine reached 100% and the yield of 1,3-cyclohexylenediamine reached 90.6% under the reaction temperature of 120°C and pressure of 5.4MPa.

[0005] At present, the research mainly uses the precious metal Ru loaded on activated carbon or alumina as a catalyst, and adds nitrate or treats the catalyst with alkali to create an alkaline environment to improve the activity of the catalyst and the selectivity for cyclohexanediamine. Precious metal catalysts have high reaction activity, but their high price limits their industrial production and application. The addition of additives also increases the separation cost. Therefore, it is of great significance to develop non-precious metal catalysts with no additives and high selectivity for the hydrogenation of m-xylylenediamine. Summary of the invention

[0006] In view of the above problems existing in the existing catalytic hydrogenation technology, the purpose of the present invention is to provide a dual non-precious metal catalyst Co-Ni / CeO2 and a preparation method thereof, as well as the application of catalyzing the selective hydrogenation of m-xylenediamine in a heterogeneous system. The catalyst uses sodium carbonate as a precipitant, loads non-precious metals Co and Ni with strong hydrogenation performance, and catalyzes the hydrogenation of m-xylenediamine without any additives. The preparation method is low in cost, the catalytic hydrogenation rate is fast, and it is easy to separate and has broad industrial prospects.

[0007] To achieve the above object, the present invention adopts the following technical solutions.

[0008] One of the purposes of the present invention is to provide a dual non-precious metal catalyst Co-Ni / CeO2, wherein Co and Ni are loaded on CeO2, wherein the total loading amount of Co and Ni is 2-8wt% of the catalyst, and the mass ratio of Co to Ni is 1:(4-0.25).

[0009] Preferably, in the above catalyst, the total loading of Co and Ni is 5wt% of the catalyst, and the mass ratio of Co to Ni is 1:1.

[0010] Another object of the present invention is to provide a method for preparing the dual non-precious metal catalyst Co-Ni / CeO2, the specific steps of which are as follows:

[0011] (1) adding cerium dioxide, cobalt nitrate hexahydrate and nickel nitrate hexahydrate into pure water and stirring them uniformly, placing the obtained suspension into a water bath at 50° C., and then adding Na2CO3 solution dropwise under vigorous stirring to adjust the pH to alkaline, stirring the obtained mixture for 2 hours, and collecting the formed precipitate;

[0012] (2) washing the collected precipitate with water, drying it in a vacuum drying oven at 60°C for 12 h, and calcining it in a muffle furnace under temperature control to obtain unreduced Co-Ni / CeO2;

[0013] (3) The unreduced Co-Ni / CeO2 is placed in a tubular furnace for temperature-controlled heating, reduced using a hydrogen-argon mixed atmosphere, naturally cooled to room temperature, and then passivated by introducing an O2 / Ar mixed gas to finally obtain a Co-Ni / CeO2 catalyst.

[0014] Preferably, in step (1), the mass ratio of cerium dioxide, cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 25:3:3.

[0015] Preferably, in step (1), Na2CO3 solution is added dropwise to adjust the pH to 9-11.

[0016] More preferably, in step (1), the pH of the solution is adjusted to 10 using Na2CO3 solution.

[0017] Preferably, in step (1), the concentration of the Na2CO3 solution is 0.1 g / mL.

[0018] Preferably, in step (2), the heating rate of the muffle furnace is 5°C / min, the calcination temperature is 250-350°C, and the calcination time is 2h.

[0019] Preferably, in step (3), the heating rate of the tubular furnace is 5°C / min, the reduction temperature in the tubular furnace is 450-550°C, and the reduction time is 2h.

[0020] Preferably, in step (3), the volume fraction of H2 in the mixed gas H2 / Ar is 5%, and the introduction time is 2 hours.

[0021] Preferably, in step (3), the volume fraction of O2 in the mixed gas O2 / Ar is 0.5%, and the introduction time is 30 minutes.

[0022] The present invention also aims to provide a dual non-precious metal catalyst Co-Ni / CeO2 for selective hydrogenation catalysis of m-xylylenediamine in a heterogeneous system. When the conversion rate of m-xylylenediamine is 100%, the selectivity of the catalyst for 1,3-cyclohexylenediamine is greater than 97%.

[0023] In order to test the catalytic performance of the dual non-precious metal catalyst Co-Ni / CeO2 of the present invention, the following method is used to verify the selective hydrogenation of m-xylylenediamine to 1,3-cyclohexylenediamine in a heterogeneous system. The specific steps are as follows:

[0024] (1) Select a stainless steel reactor;

[0025] (2) Weighing the prepared catalyst Co-Ni / CeO2 into a reaction kettle, then weighing m-xylylenediamine and dissolving it in tert-butyl alcohol solvent, and placing the mixed solution in the reaction kettle after ultrasonic dispersion;

[0026] (3) After sealing the reactor, flush it with hydrogen at a pressure of 1.0 MPa three times, maintain the hydrogen pressure at 1.0 MPa at room temperature, and check the airtightness of the reactor;

[0027] (4) Heat the reactor to 120°C, continue to introduce hydrogen to 8.0 MPa, and maintain the temperature and pressure in the reactor for 1-6 hours;

[0028] (5) After the reaction is completed, wait for the reactor to cool to room temperature, open the gas valve, and release hydrogen until the pressure is 0, completing the reaction process.

[0029] The reaction solution was filtered and then injected into a gas chromatograph. The conversion rate of the catalyst to m-xylenediamine and the selectivity of 1,3-cyclohexylenediamine were calculated by gas chromatography using n-dodecane as an internal standard.

[0030] By adopting the above technology, compared with the prior art, the beneficial effects of the present invention are as follows:

[0031] 1) The catalyst of the present invention is prepared by a deposition precipitation method, with non-precious metals as the active phase, which has a lower preparation cost than traditional precious metal catalysts, greatly reduces the cost of raw materials, and has a simple preparation process, low energy consumption, and is green and environmentally friendly;

[0032] 2) The catalyst prepared by the present invention can achieve high yield without adding additives during the reaction process, which greatly saves separation costs. The preparation method is simple and has high selectivity for the target product, and has great industrial prospects.

[0033] 3) The catalyst prepared by the present invention has high catalytic performance when the total loading is 5%. The specific conditions are that under the reaction conditions of hydrogen pressure 8MPa, temperature 120°C, reaction time 6h and catalyst 0.1g, when the conversion rate of 0.5g of m-phenylenediamine is 100%, the selectivity for 1,3-cyclohexylenediamine reaches more than 97%. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 1 is an X-ray diffraction analysis diagram of catalysts prepared in different embodiments of the present invention;

[0035] As can be seen from the figure, compared with the JCPDS standard data of cerium dioxide, elemental cobalt and elemental nickel, it can be observed that the characteristic peak of cerium dioxide is obvious, the shift of the metal diffraction peak indicates the formation of an alloy, and it is calculated that the particle size of the metal is about 20.3nm.

[0036] Figure 2 is a scanning electron microscope image of the catalyst prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0037] The technical solution of the present invention is further described below with reference to specific embodiments, but the protection scope of the present invention is not limited thereto.

[0038] The present invention uses different ratios of Co and Ni loaded on CeO2 as an example, and Co and Ni loaded on different oxide carriers as a comparative example. The specific preparation process is as follows:

[0039] (1) Using 1 g of CeO2 as a carrier, 0.1235 g of cobalt nitrate hexahydrate as a cobalt source, and 0.1238 g of nickel nitrate hexahydrate as a nickel source; cerium dioxide, cobalt nitrate hexahydrate, and nickel nitrate hexahydrate were added into pure water and stirred evenly, the obtained suspension was placed in a 50° C. water bath, and then, under vigorous stirring, Na2CO3 solution was added dropwise to adjust the pH to 10, the obtained mixture was stirred for 2 h, and the formed precipitate was collected.

[0040] (2) The collected precipitate was washed with water three times, dried in a vacuum drying oven at 60°C for 12 h, and calcined in a muffle furnace at 300°C for 2 h to obtain unreduced Co-Ni / CeO2;

[0041] (3) The unreduced catalyst Co-Ni / CeO2 was placed in a tubular furnace in a H2 / Ar atmosphere for heating reduction. The heating rate of the tubular furnace was 5°C / min, the heating temperature of the tubular furnace was 500°C, the heating time was 2h, the volume fraction of H2 in the mixed gas was 5%, and the introduction time was 2h. After naturally cooling to room temperature, an O2 / Ar mixed gas was introduced for passivation. The volume fraction of O2 was 0.5%, and the introduction time was 30min to obtain Co-Ni / CeO2.

[0042] The application process of the catalyst prepared above in the catalytic hydrogenation of m-xylylenediamine was tested, and the performance test steps were as follows:

[0043] Performance test: In a 100mL stainless steel reactor, weigh 0.1g of the catalyst Co-Ni / CeO2 into the reactor, weigh 0.5g of m-phenylenediamine and 30mL of tert-butyl alcohol, dissolve m-phenylenediamine in tert-butyl alcohol, and put the mixed solution into the reactor after ultrasonic dispersion. After sealing the reactor, flush it with hydrogen (1MPa) three times, increase the hydrogen pressure by 1MPa at room temperature, and check the air tightness; after checking the air tightness, adjust the magnetic speed to 500rpm, raise the reactor temperature to 120℃, and then introduce hydrogen until the pressure reaches 8MPa, and start timing. After reacting for 1h, when the reactor is cooled to room temperature, open the gas valve of the reactor and release hydrogen until the pressure reaches 0MPa.

[0044] After filtering the reaction solution, use a micro-injection needle to draw 0.4 μL and inject it into the gas chromatograph. The gas chromatograph hydrogen flow rate is set to 40-60 mL / min, the air flow rate is 260-300 mL / min, and the carrier gas flow rate is 2-4 mL / min. The injection temperature is set to 280.0°C, the column furnace temperature is set to 150.0°C, and the FID temperature is set to 280.0°C. Using n-dodecane as the internal standard, the conversion rate of the catalyst to m-phenylenediamine and the selectivity of 1,3-cyclohexanedimethylamine are calculated by gas chromatography.

[0045] Example 1: Application test of 5% Co-Ni / CeO2 (Co:Ni=1:1) in catalytic hydrogenation of m-xylylenediamine

[0046] The Co-Ni / CeO2 catalyst of Example 1, in which the loading amount of Co and Ni was 5% of the catalyst and the ratio of Co to Ni was 1:1, was tested in the catalytic hydrogenation of m-xylylenediamine.

[0047] Under the reaction conditions of 8 MPa hydrogen pressure, 120°C temperature, 1 h reaction, 0.1 g catalyst and 0.5 g m-xylenediamine, the catalyst conversion rate was 19.4% and the selectivity of 1,3-cyclohexylenediamine was 97.9%.

[0048] Example 2: Application test of 2% Co-Ni / CeO2 (Co:Ni=1:1) in catalytic hydrogenation of m-xylylenediamine

[0049] The Co-Ni / CeO2 catalyst of Example 2, in which the loading amount of Co and Ni is 2% of the catalyst and the ratio of Co to Ni is 1:1, was tested in the catalytic hydrogenation of m-xylylenediamine.

[0050] Under the reaction conditions of 8 MPa hydrogen pressure, 120°C temperature, 1 h reaction, 0.1 g catalyst and 0.5 g m-xylenediamine, the catalyst conversion rate was 9.4% and the selectivity of 1,3-cyclohexylenediamine was 95.2%.

[0051] Example 3: Application test of 8% Co-Ni / CeO2 (Co:Ni=1:1) in catalytic hydrogenation of m-xylylenediamine

[0052] The Co-Ni / CeO2 catalyst of Example 3, in which the loading amount of Co and Ni is 8% of the catalyst and the ratio of Co to Ni is 1:1, was tested in the catalytic hydrogenation of m-xylylenediamine:

[0053] Under the reaction conditions of 8 MPa hydrogen pressure, 120°C temperature, 1 h reaction, 0.1 g catalyst and 0.5 g m-xylenediamine, the catalyst conversion rate was 99.9% and the selectivity of 1,3-cyclohexylenediamine was 32.6%.

[0054] Example 4: Application test of 5% Co-Ni / CeO2 (Co:Ni=1:4) in catalytic hydrogenation of m-xylylenediamine

[0055] The Co-Ni / CeO2 catalyst of Example 4, in which the loading of Co and Ni was 5% of the catalyst and the ratio of Co to Ni was 1:4, was tested in the catalytic hydrogenation of m-xylylenediamine.

[0056] Under the reaction conditions of 8 MPa hydrogen pressure, 120°C temperature, 1 h reaction, 0.1 g catalyst and 0.5 g m-xylenediamine, the catalyst conversion rate was 9.3% and the selectivity of 1,3-cyclohexylenediamine was 93.6%.

[0057] Example 5: Application test of 5% Co-Ni / CeO2 (Co:Ni=4:1) in catalytic hydrogenation of m-xylylenediamine

[0058] The Co-Ni / CeO2 catalyst of Example 5, in which the loading of Co and Ni was 5% of the catalyst and the ratio of Co to Ni was 4:1, was tested in the catalytic hydrogenation of m-xylylenediamine.

[0059] Under the reaction conditions of hydrogen pressure of 4 MPa, temperature of 120°C, reaction time of 1 h, catalyst of 0.1 g and m-xylenediamine of 0.5 g, the catalyst conversion rate was 13.7% and the selectivity of 1,3-cyclohexylenediamine was 94.3%.

[0060] Comparative Example 1: Application test of 5% Co-Ni / Nb2O5 (Co:Ni=1:1) in catalytic hydrogenation of m-xylylenediamine

[0061] The Nb2O5-loaded Co-Ni / Nb2O5 catalyst of Comparative Example 1, with a loading amount of 5% for metal Co and Ni, was tested in the catalytic hydrogenation of m-xylylenediamine.

[0062] Under the reaction conditions of hydrogen pressure of 8 MPa, temperature of 120° C., reaction time of 1 h, catalyst of 0.1 g, and p-chloronitrobenzene of 0.5 g, the catalyst conversion rate was 17.1% and the selectivity of 1,3-cyclohexyldimethylamine was 89.3%.

[0063] Comparative Example 2: Application test of 5% Co-Ni / ZnO (Co:Ni=1:1) in catalytic hydrogenation of m-xylylenediamine

[0064] The ZnO-loaded Co-Ni / ZnO catalyst of Comparative Example 2, in which the metal Co and Ni loading amounts were 5% and Co:Ni=1:1, was tested in the catalytic hydrogenation of m-xylylenediamine.

[0065] Under the reaction conditions of hydrogen pressure of 8 MPa, temperature of 120°C, reaction time of 1 h, catalyst of 0.1 g, and m-phenylenediamine of 0.5 g, the catalyst conversion rate was 23.7% and the selectivity of 1,3-cyclohexylenediamine was 53.9%.

[0066] Comparative Example 3: Application test of 5% Co-Ni / SiO2 (Co:Ni=1:1) in catalytic hydrogenation of m-xylylenediamine

[0067] The SiO2-loaded Co-Ni / CeO2 catalyst of Comparative Example 3, in which the metal Co and Ni loading amounts were 5% and Co:Ni=1:1, was tested in the catalytic hydrogenation of m-xylylenediamine.

[0068] Under the reaction conditions of hydrogen pressure of 8 MPa, temperature of 120°C, reaction time of 1 h, catalyst of 0.1 g, and m-xylenediamine of 0.5 g, the catalyst conversion rate was 8.7% and the selectivity of 1,3-cyclohexylenediamine was 65.2%.

[0069] Comparative Example 4: Application test of 5% Co-Ni / ZrO2 (Co:Ni=1:1) in catalytic hydrogenation of m-xylylenediamine

[0070] The ZrO2-loaded Co-Ni / ZrO2 catalyst of Comparative Example 4, in which the metal Co and Ni loading amounts were 5% and Co:Ni=1:1, was tested in the catalytic hydrogenation of m-xylylenediamine.

[0071] Under the reaction conditions of hydrogen pressure of 8 MPa, temperature of 120°C, reaction time of 1 h, catalyst of 0.1 g, and m-phenylenediamine of 0.5 g, the catalyst conversion rate was 20.3% and the selectivity of 1,3-cyclohexylenediamine was 28.8%.

[0072] Comparative Example 5: Application test of 5% Co / CeO2 in catalytic hydrogenation of m-phenylenediamine

[0073] The catalyst Co / CeO2 in which the CeO2 of Comparative Example 5 is loaded with metal Co, wherein the loading amount of Co is 5%, is tested in the catalytic hydrogenation of m-xylylenediamine.

[0074] Under the reaction conditions of hydrogen pressure of 8 MPa, temperature of 120°C, reaction time of 1 h, catalyst of 0.1 g, and m-phenylenediamine of 0.5 g, the catalyst conversion rate was 4.9% and the selectivity of 1,3-cyclohexylenediamine was 98.1%.

[0075] Comparative Example 6: Application test of 5% Ni / CeO2 in catalytic hydrogenation of m-phenylenediamine

[0076] The catalyst Ni / CeO2 in which the CeO2 of Comparative Example 6 is loaded with metal Ni, wherein the Ni loading amount is 5%, is tested in the catalytic hydrogenation of m-xylylenediamine.

[0077] Under the reaction conditions of hydrogen pressure of 8 MPa, temperature of 120°C, reaction time of 1 h, catalyst of 0.1 g, and m-xylenediamine of 0.5 g, the catalyst conversion rate was 7.1% and the selectivity of 1,3-cyclohexylenediamine was 83.7%.

[0078] The effects of different carriers on catalytic performance were studied by comparative studies, the performance and parameters of the products were obtained by testing, and the optimal performance of the products was determined by analysis. Table 1 shows the catalyst products obtained by different carrier conditions, the results of testing their performance and the results of the comparative cases.

[0079] Table 1: Effect of different supported catalysts on hydrogenation of m-phenylenediamine

[0080]

[0081] Reaction conditions: catalyst loading of 5%, Co:Ni=1:1, catalyst 0.1 g, m-phenylenediamine 0.5 g, tert-butanol 30 mL, temperature 120°C, hydrogen pressure 8 MPa, reaction time 1 h, catalyst reducing atmosphere 5% H2 / Ar.

[0082] As can be seen from Table 1, different carriers have a great influence on the hydrogenation activity of m-phenylenediamine. Using CeO2 as a carrier can significantly improve the selectivity of 1,3-cyclohexanedimethylamine.

[0083] By studying the effect of different metal loadings on the catalytic performance of the catalyst, the performance and parameters of the product are detected, and the optimal performance of the catalyst is determined by analysis. Table 2 shows the results and comparative cases obtained by testing the performance of catalysts with different metal loadings.

[0084] Table 2: Effect of different metal loadings on catalyst activity

[0085]

[0086] Reaction conditions: Co:Ni=1:1, catalyst 0.1 g, m-xylenediamine 0.5 g, tert-butanol 30 mL, temperature 120° C., hydrogen pressure 8 MPa, reaction time 1 h.

[0087] It can be seen from Table 2 that when the metal loading is 5%, the conversion rate of m-phenylenediamine is high and the selectivity of 1,3-cyclohexanedimethylamine is also high. Therefore, 5% Co and Ni loading is the optimal loading.

[0088] By studying the effect of the loading ratio of Co and Ni on the catalytic performance of the catalyst, the performance and parameters of the product are detected, and the optimal performance of the product is determined by analysis. Table 3 shows the performance results of the catalyst products with different loading ratios of Co and Ni.

[0089] Table 3: Effect of different Co:Ni ratios on catalyst activity

[0090]

[0091] Reaction conditions: catalyst loading of 5%, catalyst 0.1 g, m-phenylenediamine 0.5 g, tert-butanol 30 mL, temperature 120° C., hydrogen pressure 8 MPa, reaction time 1 h.

[0092] It can be seen from Table 3 that when Co:Ni=1:1, the catalyst activity is higher, the yield of 1,3-cyclohexanedimethylamine is higher, and the catalytic performance is optimal.

[0093] The effect of solution pH on the performance of the catalyst during the preparation process was studied, and the optimal performance of the product was determined by analysis. Table 4 shows the effect of different solution pH on the performance of the prepared catalyst, and the performance results were tested.

[0094] Table 4: Effect of solution pH on catalytic activity

[0095]

[0096] Reaction conditions: catalyst 5% Co-Ni / CeO2 (Co:Ni=1:1) 0.1 g, m-phenylenediamine 0.5 g, tert-butanol 30 mL, temperature 120°C, hydrogen pressure 8 MPa, reducing atmosphere 5% H2 / Ar, reaction time 1 h.

[0097] It can be seen from Table 4 that the solution deposition pH has a certain influence on the catalyst activity. When the pH is less than 10, incomplete surface metal deposition may occur, resulting in low catalyst activity. When the pH is 10, it is more suitable for the attachment of the metal to the carrier, and the conversion rate of m-phenylenediamine is the highest and the selectivity of 1,3-cyclohexylenediamine is the highest.

[0098] The effect of calcination temperature on the performance of the catalyst during the preparation process was studied, and the optimal performance of the product was determined by analysis. Table 5 shows the effect of different calcination temperatures on the performance of the prepared catalyst, and the performance results were tested.

[0099] Table 5: Effect of calcination temperature on catalytic activity

[0100]

[0101] Reaction conditions: catalyst 5% Co-Ni / CeO2 (Co:Ni=1:1) 0.1 g, m-phenylenediamine 0.5 g, tert-butanol 30 mL, temperature 120°C, hydrogen pressure 8 MPa, reducing atmosphere 5% H2 / Ar, reaction time 1 h.

[0102] As can be seen from Table 5, the muffle furnace calcination temperature has a slight effect on the catalyst performance, and the catalyst performance is best when calcined at 300°C.

[0103] The effect of the reduction temperature on the performance of the catalyst during the preparation process was studied, and the optimal performance of the product was determined by analysis. Table 6 shows the effect of different heating reduction temperatures on the performance of the prepared catalyst, and the performance results were tested.

[0104] Table 6: Effect of different heating reduction temperatures on catalytic activity

[0105]

[0106]

[0107] Reaction conditions: catalyst 5% Co-Ni / CeO2 (Co:Ni=1:1) 0.1 g, m-phenylenediamine 0.5 g, tert-butanol 30 mL, temperature 120°C, hydrogen pressure 8 MPa, reducing atmosphere 5% H2 / Ar, reaction time 1 h.

[0108] It can be seen from Table 6 that when the reduction temperature is lower than 500°C, the catalyst may not be fully reduced, resulting in low activity; when the reduction temperature is 500°C, the catalyst activity is the highest; when the reduction temperature is 550°C, the catalyst surface sintered due to the high temperature, resulting in a decrease in catalyst activity.

[0109] By studying the effect of the catalytic reaction time on the catalytic performance of the catalyst during the reaction of meta-phenylenediamine, the optimal performance of the product is determined by analysis. Table 7 shows the effect of different catalytic reaction times on the performance of the catalyst, and the performance results are tested.

[0110] Table 7: Effect of reaction time on catalytic activity

[0111]

[0112]

[0113] Reaction conditions: catalyst 5% Co-Ni / CeO2 (Co:Ni=1:1) 0.1g, m-phenylenediamine 0.5g, tert-butanol 30mL, temperature 120°C, hydrogen pressure 8MPa, reducing atmosphere 5% H2 / Ar, reaction time 1-6h.

[0114] It can be seen from Table 7 that as the reaction time increases, m-phenylenediamine is completely converted in 6 h, and the selectivity of 1,3-cyclohexanedimethylamine is >97% when the reaction time is completely converted.

[0115] The above description is only part of the embodiments of the present invention and is not intended to limit the present invention. All equivalent changes and modifications made according to the content of the present invention are within the protection scope of the present invention.

Claims

1. A dual non-precious metal catalyst Co-Ni / CeO2, characterized in that: Co and Ni are loaded on CeO2, wherein the total loading amount of Co and Ni is 2-8wt% of the catalyst, and the mass ratio of Co to Ni is 1:(4-0.25).

2. The dual non-precious metal catalyst Co-Ni / CeO2 according to claim 1, characterized in that: The total loading amount of Co and Ni is 5wt% of the catalyst, and the mass ratio of Co to Ni is 1:

1.

3. A method for preparing the dual non-precious metal catalyst Co-Ni / CeO2 as described in any one of claims 1 to 2, characterized in that: The specific steps are as follows: (1) adding cerium dioxide, cobalt nitrate hexahydrate and nickel nitrate hexahydrate into pure water and stirring them uniformly, placing the obtained suspension into a water bath at 50° C., and then adding Na2CO3 solution dropwise under vigorous stirring to adjust the pH to alkaline, stirring the obtained mixture for 2 hours, and collecting the formed precipitate; (2) washing the collected precipitate with water, drying it in a vacuum drying oven at 60°C for 12 h, and calcining it in a muffle furnace under temperature control to obtain unreduced Co-Ni / CeO2; (3) The unreduced Co-Ni / CeO2 is placed in a tubular furnace for temperature-controlled heating, reduced using a hydrogen-argon mixed atmosphere, naturally cooled to room temperature, and then passivated by introducing an O2 / Ar mixed gas to finally obtain a Co-Ni / CeO2 catalyst.

4. The method for preparing the non-precious metal catalyst Co-Ni / CeO2 according to claim 3, characterized in that: In the step (1), the mass ratio of cerium dioxide, cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 25:3:

3.

5. The method for preparing the non-precious metal catalyst Co-Ni / CeO2 according to claim 3, characterized in that: In the step (1), Na2CO3 solution is added dropwise to adjust the pH to 9-11.

6. The method for preparing the non-precious metal catalyst Co-Ni / CeO2 according to claim 3, characterized in that: In the step (2), the heating rate of the muffle furnace is 5°C / min, the calcination temperature is 250-350°C, and the calcination time is 2h.

7. The method for preparing the non-precious metal catalyst Co-Ni / CeO2 according to claim 3, characterized in that: In the step (3), the heating rate of the tubular furnace is 5°C / min, the reduction temperature in the tubular furnace is 450-550°C, and the reduction time is 2h.

8. The method for preparing the non-precious metal catalyst Co-Ni / CeO2 according to claim 3, characterized in that: In the step (3), the volume fraction of H2 in the mixed gas H2 / Ar is 5%, and the introduction time is 2 hours.

9. The method for preparing the non-precious metal catalyst Co-Ni / CeO2 according to claim 3, characterized in that: In the step (3), the volume fraction of O2 in the mixed gas O2 / Ar is 0.5%, and the introduction time is 30 minutes.

10. Use of the dual non-precious metal catalyst Co-Ni / CeO2 as described in any one of claims 1 to 2 to catalyze the selective hydrogenation of m-xylylenediamine in a heterogeneous system, wherein the selectivity of the catalyst for 1,3-cyclohexylenediamine is greater than 97% when the conversion rate of m-xylylenediamine is 100%.

Citation Information

Patent Citations

  • Preparation process of 1, 3-cyclohexanediamine

    CN112479897A

  • In-situ packaging catalyst and application thereof

    CN116020456A

  • Nickel-based catalyst for hydrogenation reaction of ammonia system as well as preparation method and application of nickel-based catalyst

    CN117816171A

  • Double non-noble metal catalyst Co-Ni / La2O3, preparation method thereof and application of double non-noble metal catalyst Co-Ni / La2O3 in catalyzing selective hydrogenation of m-xylylenediamine in heterogeneous system

    CN118287087A

  • Process for producing aromatic primary diamines

    WO2016004867A1