Nitrogen-containing Y-type molecular sieve catalyst and preparation method thereof

By preparing nitrogen-containing Y-type molecular sieve catalysts, the catalyst activity attenuation problem is solved by regulating alkaline sites and transition metal salts, and the COS hydrolysis efficiency is improved and the catalyst stability is achieved. It is suitable for blast furnace gas desulfurization.

CN119076046APending Publication Date: 2024-12-06INST OF COAL CHEM CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411212048.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During the catalytic hydrolysis of COS, the alkali metals are unevenly distributed and are prone to agglomeration and loss, resulting in activity decay and unable to effectively improve the COS hydrolysis efficiency.

Method used

The preparation method of nitrogen-containing Y-type molecular sieve catalyst is adopted to form excellent hydrolysis performance by adjusting the concentration of NaOH or KOH and the silicon-aluminum ratio, and high alkaline sites are formed through transition metal salt and nitriding treatment to enhance catalytic activity.

Benefits of technology

It has achieved the improvement of COS hydrolysis conversion efficiency and the stability of the catalyst, and provided an efficient, stable and controllable catalyst design, providing technical support for blast furnace gas desulfurization in the steel industry.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a nitrogen-containing Y-type molecular sieve catalyst and a preparation method thereof. The preparation method of the nitrogen-containing Y-type molecular sieve catalyst comprises the following steps: mixing and dissolving NaOH or KOH and an aluminum source in deionized water, and stirring for 0.5-2 hours to obtain a solution A; adding a silicon source into deionized water, and stirring for 0.5-2 hours to obtain a solution B; mixing the solution A and the solution B, stirring for 0.5-4 hours to obtain a precursor solution C, and then performing ultrasonic oscillation and aging for 0.5-48 hours to obtain D; placing the obtained D in a hydrothermal kettle for reaction, after the reaction is finished, performing centrifugal separation, washing to be neutral, and then drying to obtain a Y-type molecular sieve; and placing the Y-type molecular sieve in a tubular furnace, introducing NH3 by taking N2 as a carrier gas, heating for heat treatment, and then cooling to room temperature. The nitrogen-containing Y-type molecular sieve catalyst is prepared by the preparation method, and is suitable for catalytic hydrolysis of COS. The method provided by the invention is low in cost, simple to operate and easy to popularize, and the prepared nitrogen-containing Y-type molecular sieve catalyst is high in COS catalytic hydrolysis conversion rate and strong in stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and in particular relates to a nitrogen-containing Y-type molecular sieve catalyst and a preparation method thereof. Background Art

[0002] Fine desulfurization of blast furnace gas is the key to achieving ultra-low emissions in the entire process of multiple processes in the steel industry. Organic sulfur, mainly carbonyl sulfide (COS), accounts for the highest proportion in blast furnace gas, and is the top priority of fine desulfurization at the source. Selecting catalytic hydrolysis of COS to convert it into inorganic sulfur (COS+H2O→H2S+CO2), and then removing inorganic sulfur by dry method is the optimal route to achieve fine desulfurization at the source. The hydrolysis of COS is a typical solid base catalytic reaction. The weak alkaline center (-OH) and medium-strong alkaline center (MO) in the solid base are the main active sites involved in the hydrolysis reaction. Avoiding the interaction between the two active sites and other impurities in the gas is an effective strategy to improve the stability of the catalyst. Commonly used hydrolysis catalysts use metal oxides such as Al2O3 and TiO2 as carriers, and load alkali metals and (or) alkaline earth metals to adjust the strength and abundance of the alkaline center, and have high hydrolysis activity. However, the alkali metals are distributed on the surface of the carrier, and are easy to agglomerate and lose during the hydrolysis process, resulting in a significant attenuation of activity. CN202211732096 loads AgY molecular sieve on the surface of alumina, which enhances the adsorption performance of inorganic sulfur H2S and avoids H2S consuming hydrolysis active sites, but does not mention that it has catalytic hydrolysis activity.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] The object of the present invention is to provide a nitrogen-containing Y-type molecular sieve catalyst and a preparation method thereof to solve the above problems.

[0005] In order to achieve the above objectives, the present invention particularly adopts the following technical solutions:

[0006] A method for preparing a nitrogen-containing Y-type molecular sieve catalyst comprises the following steps:

[0007] S1: Dissolve NaOH or KOH and an aluminum source in deionized water and stir for 0.5 to 2 hours to obtain solution A; the aluminum source includes Al(OH)3, NaAlO2, Al2(SO4)3, C9H 21 AlO3; Preferably, the molar ratio of the NaOH or KOH to the aluminum source is 5:1 to 20:1.

[0008] S2: Add a silicon source into an appropriate amount of deionized water and stir for 0.5h to 2h to obtain solution B; the silicon source includes Na2SiO3, NaAlSiO3, and SiO2; preferably, the molar ratio of the silicon source to the aluminum source is 5:1 to 20:1.

[0009] First, the alkalinity of the molecular sieve is adjusted by adjusting the concentration of NaOH or KOH. The concentration of silicon is mainly related to the strength of the molecular sieve. The strength of the molecular sieve is regulated by adjusting the amount of silicon and aluminum. At the same time, the silicon-aluminum ratio will also affect the acidity and alkalinity of the molecular sieve itself, thereby further controlling its excellent hydrolysis performance.

[0010] S3: Mix solution A obtained in S1 and solution B obtained in S2, stir for 0.5 h to 4 h to obtain precursor solution C, and then ultrasonically oscillate and age for 0.5 h to 48 h to obtain D;

[0011] S4: placing D obtained in S3 in a hydrothermal autoclave for reaction, centrifugally separating and washing to neutrality after the reaction, and then drying to obtain a Y-type molecular sieve; the reaction temperature is 50-200°C, and the time is 2-30h; the drying temperature is 100-110°C, and the time is 6-12h.

[0012] Before step S5, the Y-type molecular sieve obtained in step S4 is immersed in a transition metal salt solution, stirred for 10 to 24 hours, then washed, filtered, dehydrated, and calcined at 450 to 600° C. for 2 to 5 hours, and the calcined product is subjected to the heat treatment described in step S5.

[0013] The transition metal salt includes a water-soluble salt of Zn, Mg, Ni, Fe, Co or Cu; preferably, the concentration of the transition metal salt solution is 0.2-1 mol / L; preferably, each gram of the Y-type molecular sieve is immersed in 10-80 mL of the transition metal salt solution.

[0014] The concentration and dosage of transition metals will also affect the alkalinity of the molecular sieve. These metals bond with O to form medium-strong alkaline centers, so their concentration is directly related to the abundance and strength of the overall alkaline sites of the molecular sieve. The preferred types and concentrations of transition metal salts in this application make the abundance and strength of the molecular sieve reach a more comprehensive state.

[0015] S5: placing the Y-type molecular sieve obtained in S4 in a tubular furnace, introducing NH3 with N2 as carrier gas, heating to 750-1000° C. for heat treatment, and then cooling to room temperature to obtain the nitrogen-containing Y-type molecular sieve catalyst.

[0016] Preferably, the heat treatment time is 6 to 10 hours; the heat treatment temperature is 750 to 1000° C., and the NH 3 flow rate is 600 ml / min or more.

[0017] Preferably, in the step S5, before the heat treatment, the process further comprises controlling the NH3 flow rate to 100 ml / min or less and performing pretreatment at 200-350°C; the pretreatment time is 0.5 to 2 hours.

[0018] The present invention replaces part of the oxygen atoms in the molecular sieve framework with nitrogen atoms through high-temperature heat treatment. The obtained novel molecular sieve catalyst with heteroatoms (nitrogen atoms) in the framework retains the inherent characteristics of conventional molecular sieve catalysts such as high specific surface area, high stability and facilitation of molecular adsorption and diffusion, while also having alkaline catalytic functions with adjustable alkalinity and shape selectivity.

[0019] In particular, NaY type molecular sieves have abundant weak alkaline sites (-OH). After ion exchange modification of NaY molecular sieves, the interaction between metal ions and S atoms in COS is enhanced. After nitridation treatment, some O atoms in the framework are replaced by N atoms, the alkalinity strength and sites are further optimized, and the COS hydrolysis activity is improved. Moreover, thanks to the high hydrothermal stability of the molecular sieve itself, the nitrided molecular sieve has excellent stability during the hydrolysis process.

[0020] Before heat treatment, pretreatment at 200-350°C can create defects to increase the nitrogen content during nitrogen doping. Pretreatment before heat treatment can create more unsaturated sites to provide sites for subsequent nitrogen doping, thereby increasing the overall nitrogen content and further adjusting the abundance of basic sites, which is beneficial to the adsorption and hydrolysis of COS.

[0021] The invention provides a nitrogen-containing Y-type molecular sieve catalyst, which is prepared by the preparation method; the nitrogen-containing Y-type molecular sieve catalyst is suitable for catalytic hydrolysis of COS.

[0022] Beneficial effects of the present invention:

[0023] The preparation method provided by the invention has the advantages of simple operation, simple and controllable conditions, cheap and readily available raw materials, green and environmentally friendly process, high technical repeatability and high yield, and is convenient for industrial promotion and use.

[0024] The prepared nitrogen-containing Y-type molecular sieve catalyst has high catalytic hydrolysis conversion efficiency and excellent stability for COS, and can provide a reference for the design and construction of efficient and stable COS hydrolysis catalysts. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1

[0027] According to the preparation method of the nitrogen-containing Y-type molecular sieve catalyst provided by the present invention, the specific steps are as follows:

[0028] S1: Weigh NaOH and Al2(SO4)3 in a molar ratio of 5:1, dissolve in water and stir for 0.5h to obtain solution A;

[0029] S2: weigh NaAlSiO3, the molar ratio of which to Al2(SO4)3 is 8:1, dissolve in water and stir for 0.5h to obtain solution B;

[0030] S3: The obtained solutions A and B are mixed and stirred for 1 hour to obtain a precursor solution C, which is then ultrasonically vibrated and aged for 2 hours to obtain D;

[0031] S4: Move the D obtained in S3 to a hydrothermal reactor for reaction for 3 hours, set the reaction temperature to 150°C, and after the reaction is completed, take it out and centrifuge it, wash it with deionized water until it is neutral, and dry it at 110°C for 6 hours to obtain a NaY type molecular sieve;

[0032] S5: The NaY molecular sieve obtained in S4 is placed in a prepared Zn(NO3)2 solution with a concentration of 0.5 mol / L, stirred in a water bath for 10 h, then washed, filtered and dehydrated, and then calcined at 600°C for 2 h. The obtained material is marked as ZnY;

[0033] S6: Place ZnY in a tubular furnace, introduce NH3 using N2 as a carrier gas, raise the temperature to 750°C, heat treat for 10 hours, cool to room temperature, and take out to obtain a nitrogen-containing ZnY molecular sieve.

[0034] Example 2

[0035] According to the preparation method of the nitrogen-containing Y-type molecular sieve catalyst provided by the present invention, the specific steps are as follows:

[0036] S1: Weigh NaOH and Al2(SO4)3 in a molar ratio of 10:1, dissolve in water and stir for 1 h to obtain solution A;

[0037] S2: Weigh NaAlSiO3 in a molar ratio of 15:1 to Al2(SO4)3, dissolve in water and stir for 1 h to obtain solution B;

[0038] S3: The obtained solutions A and B are mixed and stirred for 2 hours to obtain a precursor solution C, which is then ultrasonically vibrated and aged for 20 hours to obtain D;

[0039] S4: Move the D obtained in S3 to a hydrothermal reactor for reaction for 2 hours, set the reaction temperature to 90°C, and after the reaction is completed, take it out and centrifuge it, wash it with deionized water until it is neutral, and dry it at 110°C for 8 hours to obtain a NaY type molecular sieve;

[0040] S5: The NaY molecular sieve obtained in S4 is placed in a prepared Zn(NO3)2 solution with a concentration of 0.2 mol / L, stirred in a water bath for 12 h, then washed, filtered and dehydrated, and then calcined at 500°C for 3 h. The obtained material is marked as ZnY;

[0041] S6: Place ZnY in a tubular furnace, introduce NH3 using N2 as a carrier gas, raise the temperature to 900°C, heat treat for 6 hours, cool to room temperature, and take out to obtain a nitrogen-containing ZnY molecular sieve.

[0042] Example 3

[0043] According to the preparation method of the nitrogen-containing Y-type molecular sieve catalyst provided by the present invention, the specific steps are as follows:

[0044] S1: Weigh NaOH and Al2(SO4)3 in a molar ratio of 18:1, dissolve in water and stir for 1 h to obtain solution A;

[0045] S2: Weigh NaAlSiO3 in a molar ratio of 10:1 to Al2(SO4)3, dissolve in water and stir for 0.5 h to obtain solution B;

[0046] S3: The obtained solutions A and B are mixed and stirred for 1 hour to obtain a precursor solution C, which is then ultrasonically vibrated and aged for 2 hours to obtain D;

[0047] S4: Move the D obtained in S3 to a hydrothermal reactor and react for 3 hours. Set the reaction temperature to 180°C. After the reaction is completed, take it out and centrifuge it, wash it with deionized water until it is neutral, and dry it at 110°C for 6 hours to obtain a NaY type molecular sieve;

[0048] S5: The NaY molecular sieve obtained in S4 is placed in a prepared Zn(NO3)2 solution with a concentration of 0.8 mol / L, stirred in a water bath for 10 h, then washed, filtered and dehydrated, and then calcined at 450°C for 5 h. The obtained material is marked as ZnY;

[0049] S6: Place ZnY in a tubular furnace, introduce NH3 using N2 as a carrier gas, heat to 800°C, heat treat for 8 hours, cool to room temperature, and take out to obtain a nitrogen-containing ZnY molecular sieve.

[0050] Example 4

[0051] The difference from Example 1 is that S5 is not included, and the S4 product NaY type molecular sieve is directly placed in a tubular furnace, NH3 is introduced with N2 as the carrier gas, the temperature is raised to 750°C, and after heat treatment for 10 hours, it is cooled to room temperature and taken out to obtain the nitrogen-containing Y type molecular sieve.

[0052] Example 5

[0053] The difference from Example 4 is that the S4 product NaY type molecular sieve is placed in a tubular furnace, first pretreated and then heat treated, and the specific conditions are set as follows: first set the NH3 flow rate to 90 ml / min, raise the temperature to 300°C, pretreat for 1 hour, then set the NH3 flow rate to 600 ml / min, and raise the temperature to 750°C. After heat treatment for 10 hours, cool to room temperature and take out to obtain the nitrogen-containing Y type molecular sieve.

[0054] Example 6

[0055] According to the preparation method of the nitrogen-containing Y-type molecular sieve catalyst provided by the present invention, the specific steps are as follows:

[0056] S1: Same as Example 1;

[0057] S2: Same as Example 1;

[0058] S3: Same as Example 1;

[0059] S4: Same as in Example 1;

[0060] S5: Same as in Example 1;

[0061] S6: Place ZnY in a tubular furnace, introduce NH3 using N2 as the carrier gas, first set the NH3 flow rate to 90 ml / min, raise the temperature to 300°C, pretreat for 1 hour, then set the NH3 flow rate to 600 ml / min, and raise the temperature to 750°C. After heat treatment for 10 hours, cool to room temperature and take out to obtain the nitrogen-containing ZnY molecular sieve.

[0062] Comparative Example 1

[0063] S1: Weigh NaOH and Al2(SO4)3 in a molar ratio of 5:1, dissolve in water and stir for 0.5h to obtain solution A;

[0064] S2: weigh NaAlSiO3, the molar ratio of which to Al2(SO4)3 is 8:1, dissolve in water and stir for 0.5h to obtain solution B;

[0065] S3: The obtained solutions A and B are mixed and stirred for 1 hour to obtain a precursor solution C, which is then ultrasonically vibrated and aged for 2 hours to obtain D;

[0066] S4: Move the D obtained in S3 to a hydrothermal reactor for reaction for 3 hours, set the reaction temperature to 150°C, and after the reaction is completed, take it out and centrifuge it, wash it with deionized water until it is neutral, and dry it at 110°C for 6 hours to obtain a NaY type molecular sieve;

[0067] S5: Grind and mix NaY molecular sieve and γ-alumina powder thoroughly, with the mass ratio of NaY to alumina being 1:9, to obtain a composite catalyst.

[0068] Comparative Example 2

[0069] S1: Weigh NaOH and Al2(SO4)3 in a molar ratio of 5:1, dissolve in water and stir for 0.5h to obtain solution A;

[0070] S2: weigh NaAlSiO3, the molar ratio of which to Al2(SO4)3 is 8:1, dissolve in water and stir for 0.5h to obtain solution B;

[0071] S3: The obtained solutions A and B are mixed and stirred for 1 hour to obtain a precursor solution C, which is then ultrasonically vibrated and aged for 2 hours to obtain D;

[0072] S4: Move the D obtained in S3 to a hydrothermal reactor for reaction for 3 hours, set the reaction temperature to 150°C, and after the reaction is completed, take it out and centrifuge it, wash it with deionized water until it is neutral, and dry it at 110°C for 6 hours to obtain a NaY type molecular sieve;

[0073] S5: Grind and mix NaY molecular sieve and γ-alumina powder thoroughly, with the mass ratio of NaY to alumina being 1:9, to obtain a composite catalyst;

[0074] S6: The composite catalyst obtained in S5 is immersed in a saturated zinc nitrate solution for 12 hours, filtered, washed with water, and dried to obtain a transition metal-modified composite catalyst.

[0075] When the catalysts provided in the examples and comparative examples are used to catalyze the hydrolysis of COS, at a temperature of 100°C and a space velocity of 10000 h -1 、COS concentration 180mg / m 3 Under the following conditions, the COS hydrolysis conversion rate (%) is shown in Table 1:

[0076] Table 1. Test results of COS hydrolysis conversion rate catalyzed by the catalysts provided in the examples and comparative examples

[0077] project 1h 5h 10h 15h 20h Example 1 95.0 93.1 92.3 90.5 91.2 Example 2 92.5 90.1 89.3 89.5 90.1 Example 3 91.5 89.2 89.3 90.0 89.5 Example 4 94.2 92.5 92.0 89.7 90.1 Example 5 95.5 94.2 93.4 92.9 92.9 Example 6 98.5 98.6 99.1 98.9 98.5 Comparative Example 1 79.6 78.9 75.6 75.7 75.0 Comparative Example 2 85.7 85.5 82.3 84.1 81.9

[0078] According to Table 1, under the same test conditions, the hydrolysis conversion rate of COS catalyzed by the nitrogen-containing Y-type molecular sieve catalyst provided in the present application is generally higher than that of the comparative example and the prior art, and the conversion rate does not show a significant decrease over time, indicating that it has good stability.

[0079] At the same time, it can be seen from Examples 1 and 4 that the COS hydrolysis conversion rate of the nitrogen-containing Y-type molecular sieve obtained by loading the transition metal on the Y-type molecular sieve and then nitrogen doping is further improved; through the comparison of Examples 4 and 5, and Examples 1 and 6, it can be seen that regardless of whether the transition metal is pre-loaded or not, pretreatment and then heat treatment are performed during the nitrogen doping process of the Y-type molecular sieve, which can significantly improve the catalytic activity of the obtained product.

[0080] Surface alkalinity is a key factor affecting the activity of carbonyl sulfide hydrolysis. The present application forms alkaline sites with different base strengths on the catalyst surface by doping nitrogen, loading transition metals, etc., thereby significantly improving the COS hydrolysis performance.

[0081] Please note that the technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. The above embodiments only express several implementation methods of the present application, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several variations and improvements can be made, which all belong to the scope of protection of the present application. Therefore, the scope of protection of the patent in this application shall be based on the attached claims.

Claims

1. A method for preparing a nitrogen-containing Y-type molecular sieve catalyst, characterized in that: The steps include: S1: Dissolve NaOH or KOH and aluminum source in deionized water and stir for 0.5h to 2h to obtain solution A; S2: Add the silicon source into an appropriate amount of deionized water and stir for 0.5h to 2h to obtain solution B; S3: Mix solution A obtained in S1 and solution B obtained in S2, stir for 0.5 h to 4 h to obtain precursor solution C, and then ultrasonically oscillate and age for 0.5 h to 48 h to obtain D; S4: placing the D obtained in S3 in a hydrothermal reactor for reaction, centrifugally separating and washing to neutrality after the reaction, and then drying to obtain a Y-type molecular sieve; S5: placing the Y-type molecular sieve obtained in S4 in a tubular furnace, introducing NH3 with N2 as carrier gas, heating up for heat treatment, and then cooling to room temperature to obtain the nitrogen-containing Y-type molecular sieve catalyst.

2. The preparation method according to claim 1, characterized in that: The aluminum source includes Al(OH)3, NaAlO2, Al2(SO4)3, C9H 21 AlO3; Preferably, the molar ratio of the NaOH or KOH to the aluminum source is 5:1 to 20:

1.

3. The preparation method according to claim 1 or 2, characterized in that: The silicon source includes Na2SiO3, NaAlSiO3, and SiO2; Preferably, the molar ratio of the silicon source to the aluminum source is 5:1 to 20:

1.

4. The preparation method according to claim 1, characterized in that: In step S4, the reaction temperature is 50-200° C. and the reaction time is 2-30 hours; Preferably, the drying temperature is 100-110° C. and the drying time is 6-12 hours.

5. The preparation method according to claim 1, characterized in that: In the step S5, the target temperature of the heating is 750-1000°C; Preferably, the heat treatment time is 6 to 10 hours.

6. The preparation method according to claim 1, characterized in that: In the step S5, before the heat treatment, the NH3 flow rate is controlled to be 100 ml / min or less, and pretreatment is performed at 200-350°C; Preferably, the pretreatment time is 0.5 to 2 hours.

7. The preparation method according to claim 5 or 6, characterized in that: The temperature of the heat treatment is 750-1000° C., and the NH 3 flow rate is 600 ml / min or above.

8. The preparation method according to claim 1 or 6, characterized in that: Before step S5, the Y-type molecular sieve obtained in step S4 is immersed in a transition metal salt solution, stirred for 10 to 24 hours, then washed, filtered, dehydrated, and calcined at 450 to 600° C. for 2 to 5 hours, and the calcined product is subjected to the heat treatment described in step S5.

9. The preparation method according to claim 8, characterized in that: The transition metal salt includes a water-soluble salt of Zn, Mg, Ni, Fe, Co or Cu; Preferably, the concentration of the transition metal salt solution is 0.2 to 1 mol / L; Preferably, each gram of the Y-type molecular sieve is immersed in 10 to 80 mL of the transition metal salt solution.

10. A nitrogen-containing Y-type molecular sieve catalyst, characterized in that: Prepared by the preparation method according to any one of claims 1 to 9; The nitrogen-containing Y-type molecular sieve catalyst is suitable for catalytic hydrolysis of COS.