Photo-thermal super-hydrophobic coating as well as preparation method and application thereof

Through the combination of micro-nanoimprinting technology and specific materials, a photothermal superhydrophobic coating with gradient distribution photothermal fillers was prepared, which solved the problem of insufficient photothermal conversion capability of the existing photothermal superhydrophobic coating, and achieved efficient and stable Deicing effect and durability.

CN119076341APending Publication Date: 2024-12-06GUANGXI LIUGONG METATHINGS TECHNOLOGY CO LTD +2

Patent Information

Application Number
CN202411207036.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing photothermal superhydrophobic coatings have insufficient photothermal conversion capabilities, low utilization rate, poor stability and aging resistance, resulting in short service life and difficulty in large-scale production.

Method used

Micro-nanoimprinting technology combined with specific materials and processes to prepare superhydrophobic surfaces with directional arrangement of micro-nano structures, and form gradient distribution photothermal fillers in the coating to improve photothermal conversion performance and stability, and through laser etching The template is obtained and microstructures are transferred to achieve large-scale preparation.

Benefits of technology

It achieves efficient photothermal conversion performance and UV aging resistance, extends service life, improves light utilization and photothermal conversion efficiency, has long-term and stable deicing effect, and reduces production costs and time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076341A_ABST
    Figure CN119076341A_ABST
Patent Text Reader

Abstract

The invention provides a photo-thermal super-hydrophobic coating and a preparation method and application thereof, and the preparation method comprises the following steps: carrying out laser etching on a metal substrate to obtain a template with a microstructure on the surface; coating the matrix with an epoxy coating, and performing first drying to obtain a first coating; coating the first coating with a photo-thermal hydrophobic coating, and performing secondary drying to obtain a photo-thermal coating; the photo-thermal hydrophobic coating comprises epoxy resin, a curing agent, a photo-thermal filler and a fluorine-containing silane coupling agent, a template is arranged on the photo-thermal coating, the microstructure on the surface of the template makes contact with the photo-thermal coating, and then the photo-thermal super-hydrophobic coating is obtained through extrusion, template removal and third drying. The super-hydrophobic surface with the directionally-arranged micro-nano structure is prepared through the design and combination of the micro-nano imprinting technology, the specific materials and the process, and the photo-thermal filler in gradient distribution is formed, so that the super-hydrophobic surface has excellent photo-thermal conversion performance and aging resistance, and excellent active and passive deicing effects are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of super-hydrophobic coatings, and in particular relates to a photothermal super-hydrophobic coating and a preparation method and application thereof. Background Art

[0002] With the rapid development of modern science and technology, there are many types of outdoor high-voltage antennas, high towers, high-altitude aircraft, etc. However, due to the influence of weather, the surface is prone to frost and ice, which brings many inconveniences to people's production and life. For example, ice will pose a major threat to flight safety belts, and aircraft icing has caused huge losses of life and property many times; in winter, the water inside the water supply corridor will easily cause the HDPE pipe water meter joint to swell and crack after freezing; air conditioners, refrigerators, and large wind turbines will cause huge power consumption. In response to these problems, researchers have proposed a series of anti-icing and de-icing methods, among which the earlier and most widely used ones are active anti-icing methods with the help of external forces, such as mechanical de-icing, thermal de-icing, and chemical de-icing, but such methods are costly, energy-intensive, and inefficient, and there is a risk of polluting the ecological environment.

[0003] Due to the super-hydrophobicity and self-cleaning properties of the lotus leaf surface, water strider and dragonfly limbs, the "lotus effect" exhibited by the surface of insects, such as lotus leaves, water striders and dragonflies, super-hydrophobic coating materials have broad application prospects in aerospace, military, transportation, construction and other fields, and have also been used in anti-icing technology in recent years. Compared with active anti-icing technology that requires external force, the excellent water repellency of super-hydrophobic surfaces enables passive anti-icing without consuming external energy, thus attracting widespread attention.

[0004] Super-hydrophobic coatings are mainly divided into two types, one is to trap air in a rough structure on the surface, reducing the solid-liquid contact area, and the other is to use low surface energy materials to reduce surface energy and reduce the adhesion between solid and liquid. For example, CN116333592A discloses a transparent super-hydrophobic deicing coating, including a carrier and a super-hydrophobic layer located on the carrier, wherein the super-hydrophobic layer has a micro-nano structure formed by polydimethylsiloxane micron particles and metal oxide nanoparticles, wherein the metal oxide nanoparticles are zinc oxide or tin oxide, and have a high transparency while meeting the super-hydrophobic performance. However, deicing by relying solely on super-hydrophobic properties has certain limitations, and the passive anti-icing effect is not ideal, and it is difficult to meet the various application requirements in different scenarios.

[0005] In order to make up for the performance defects of super-hydrophobic anti-icing, researchers have proposed a technology that combines photothermal effect with super-hydrophobic surface. This technology combines the advantages of active anti-icing and passive anti-icing, and can play a role in various stages of the icing process. It not only exhibits anti-icing performance, but also due to the photothermal effect, the ice on the coating surface can be quickly melted under light conditions. For example, CN111073450A discloses a method for preparing an active photothermal deicing coating with super-hydrophobic properties, including the following steps: coating polydimethylsiloxane on the surface of a substrate and letting it stand; coating or spraying an active photothermal deicing coating with super-hydrophobic properties on the polydimethylsiloxane, drying, and obtaining an active photothermal deicing coating with super-hydrophobic properties; the active photothermal deicing coating includes components such as epoxy resin, fluoropolymer, silicon carbide, carbon nanotubes and solvent. CN113667400A discloses a method for preparing an anti-icing and deicing coating having both photothermal and self-cleaning properties, comprising the following steps: adding dodecylamine to a multi-walled carbon nanotube dispersion to obtain a dispersion B; adding dopamine to the dispersion B, stirring and filtering, and drying to obtain a carbon nanotube modified with super-hydrophobic polydopamine PDA, and then mixing it with a thermosetting resin, a curing agent, etc. to form a slurry; spraying the slurry on a substrate, and curing to obtain an anti-icing and deicing coating. Although the surface of the existing photothermal super-hydrophobic coating can play a certain anti-icing and deicing role, the photothermal conversion capacity is insufficient, especially the utilization rate of light is low, and the stability and aging resistance of the coating are low at the same time, and it is easy to age in an ultraviolet environment, and the service life is short, and there is a large difficulty in large-scale use. Therefore, it is a problem to be solved in this field to develop a photothermal super-hydrophobic material with high photothermal conversion efficiency, good stability and aging resistance, long service life, and easy large-scale preparation. Summary of the invention

[0006] In view of the deficiencies in the prior art, the object of the present invention is to provide a photothermal super-hydrophobic coating and a preparation method and application thereof. By introducing micro-nano imprinting technology and combining it with specific materials and processes, a super-hydrophobic surface with a directionally arranged micro-nano structure can be prepared, so that a gradient-distributed photothermal filler is formed in the photothermal super-hydrophobic coating. While having excellent photothermal conversion performance, it has good stability and aging resistance, a long service life, and can achieve long-term and stable active and passive deicing effects.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a method for preparing a photothermal super-hydrophobic coating, the preparation method comprising the following steps:

[0009] Laser etching the metal substrate to obtain a template with a microstructure on the surface;

[0010] Applying epoxy coating on the substrate and first drying to obtain a first coating;

[0011] Applying a photothermal hydrophobic coating on the first coating, and drying the coating to obtain a photothermal coating; the photothermal hydrophobic coating comprises a combination of an epoxy resin, a curing agent, a photothermal filler and a fluorine-containing silane coupling agent;

[0012] The template is arranged on the photothermal coating so that the microstructure on the surface of the template contacts the photothermal coating, and then the photothermal super-hydrophobic coating is obtained through extrusion, template removal and third drying.

[0013] The preparation method provided by the present invention introduces micro-nano imprinting technology, and the template imprinting method can be used to realize large-scale preparation of super-hydrophobic surfaces with directional arranged micro-nano structures, which has the advantages of good repeatability, low cost, high structural resolution, etc.; since the micro-nano imprinting technology uses laser etching to obtain a template with a microstructure and transfers the pattern by mechanical means, it can achieve extremely high resolution; at the same time, the template with a microstructure on the surface can be used repeatedly, which greatly reduces the processing cost and effectively shortens the processing time.

[0014] The present invention sequentially prepares a first coating without photothermal fillers and a photothermal coating containing photothermal fillers on a substrate, and after extrusion, demoulding and drying, a photothermal super-hydrophobic coating with a photothermal filler concentration gradient can be obtained, realizing a gradient effect of increasing photothermal filler concentration from the substrate to the coating surface, thereby achieving the purpose of deicing based on photothermal conversion. Since the application of photothermal fillers itself will bring internal defects to the coating, the present invention designs a low content of photothermal fillers near the coating close to the substrate, most of which is the combination of epoxy coating and substrate, so the coating has fewer internal defects and better bonding with the substrate; the coating surface has a higher concentration of photothermal fillers, which enhances the photothermal conversion performance of the coating itself; at the same time, micro-nano imprinting technology can form a rich micro-nano (inverted triangle) structure on the coating surface, which greatly enhances the multiple scattering of light particles, so that light energy can be used multiple times and converted into heat energy, further enhancing the utilization rate of light and the photothermal conversion efficiency.

[0015] In addition, since epoxy resin is in an excited state under the action of ultraviolet light, it is decomposed into free radicals and reacts with oxygen to generate hydroperoxides, and finally a series of molecular chain breaks or crosslinks are triggered; In addition, the unsaturated bonds such as benzene rings contained in epoxy resin, polar groups such as ether bonds, and impurities introduced during the polymerization stage and processing, etc., easily absorb ultraviolet rays to produce initiation, resulting in photo-oxidation of epoxy resin. During the photo-oxidation aging process of epoxy resin, the number of carbonyl chromophores continues to increase, and yellowing occurs on the resin surface. The present invention designs a coating structure with a concentration gradient of photothermal fillers, and the abundant photothermal fillers on the coating surface can reduce the energy density of ultraviolet light during photothermal conversion, weaken the photo-oxidation reaction of epoxy resin, and improve the aging resistance and service life of the photothermal super-hydrophobic coating.

[0016] Therefore, the present invention is designed and combined with each other by micro-nano imprinting technology, specific materials, and preparation technology, so that the obtained photothermal super-hydrophobic coating has a super-hydrophobic surface of directional arrangement micro-nano structure, and a photothermal filler with gradient distribution is formed in the coating at the same time, so as to realize excellent active deicing and passive deicing effects based on super-hydrophobic properties and photothermal conversion performance, and improve light utilization rate and photothermal conversion efficiency; The photothermal super-hydrophobic coating has good stability and UV aging resistance, suppresses yellowing, and has a long service life, and can achieve long-term stable active and passive deicing effects. The preparation method has the characteristics of good repeatability, low cost, and easy to realize large-scale production, and has broad application prospects.

[0017] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.

[0018] As a preferred technical solution of the present invention, a metal substrate is placed on a laser processing work platform and laser etching is performed to obtain a template with a microstructure on the surface.

[0019] Due to the hydrophobicity of traditional super-hydrophobic surface structure, most of them are prepared by spraying, and the prepared surface microstructure presents an irregular non-directional arrangement structure, and this structure cannot accurately control the microstructure spacing and microstructure arrangement uniformity, resulting in uneven distribution of super-hydrophobic surface microstructures, and performance is different. In the freezing process, it is easy to change from the Cassie-Baxter model to the Wenzel model, and in the process of repeatedly freezing and melting ice, the region with a larger structure spacing is easily invalidated, resulting in undesirable super-hydrophobic performance, easy adhesion of water droplets, causing ice and super-hydrophobic surface adhesion to increase, and deicing failure. The present invention uses laser etching to obtain a regular microstructure with periodicity and directional arrangement, and then by extrusion (micro-nano embossing / embossing), the regular microstructure is transferred to the photothermal coating, so that the photothermal super-hydrophobic coating has a super-hydrophobic surface with a directional arrangement microstructure, and it is possible to achieve the preparation of planning, and the template can be repeatedly reused, effectively reducing processing costs, shortening processing time, and improving production efficiency.

[0020] It should be noted that the shapes of the template, metal substrate and substrate (and the photothermal coating formed thereon) in the present invention match each other so as to transfer the microstructure on the template to the photothermal coating. The surface of the substrate can be a plane, and the metal substrate and the template formed therefrom also include a plane structure (a template with a microstructure on a plane surface); the surface of the substrate can also be a curved surface, and the metal substrate and the template formed therefrom also include a curved surface (a template with a microstructure on a curved surface surface), and the template can have variability and plasticity according to the adaptation with the substrate.

[0021] Preferably, the metal substrate comprises a stainless steel plate.

[0022] Preferably, the metal substrate is pretreated before laser etching, and the pretreatment includes grinding and rust removal, ultrasonic cleaning and oil removal, and pickling and activation performed in sequence.

[0023] Preferably, the temperature of the ultrasonic cleaning and oil removal is 60-80°C, for example, it can be 62°C, 65°C, 68°C, 70°C, 72°C, 75°C or 78°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0024] Preferably, the ultrasonic cleaning and oil removal time is 5-15 minutes, for example, it can be 6 minutes, 8 minutes, 10 minutes, 12 minutes or 14 minutes, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0025] Preferably, the degreasing agent used in the ultrasonic cleaning comprises a combination of sodium hydroxide, sodium carbonate, sodium phosphate and an emulsifier.

[0026] Preferably, the concentration of sodium hydroxide in the degreasing agent is 40-60 g / L, for example, it can be 42 g / L, 45 g / L, 48 g / L, 50 g / L, 52 g / L, 55 g / L or 58 g / L, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0027] Preferably, the concentration of sodium carbonate in the degreasing agent is 30-60 g / L, for example, it can be 32 g / L, 35 g / L, 38 g / L, 40 g / L, 42 g / L, 45 g / L, 48 g / L, 50 g / L, 52 g / L, 55 g / L or 58 g / L, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0028] Preferably, the concentration of sodium phosphate in the degreasing agent is 30-60 g / L, for example, it can be 32 g / L, 35 g / L, 38 g / L, 40 g / L, 42 g / L, 45 g / L, 48 g / L, 50 g / L, 52 g / L, 55 g / L or 58 g / L, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0029] Preferably, the emulsifier comprises OP-10 emulsifier.

[0030] Preferably, the concentration of the emulsifier in the deoiling agent is 2-6 mL / L, for example, it can be 2.5 mL / L, 3 mL / L, 3.5 mL / L, 4 mL / L, 4.5 mL / L, 5 mL / L or 5.5 mL / L, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0031] Preferably, the acid solution used for the pickling activation comprises dilute sulfuric acid and / or dilute hydrochloric acid, and dilute sulfuric acid is more preferred.

[0032] Preferably, the acid concentration in the acid solution is 0.5-1.5 mol / L, for example, it can be 0.6 mol / L, 0.8 mol / L, 1 mol / L, 1.2 mol / L or 1.4 mol / L, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0033] Preferably, the acid pickling activation temperature is 15-40°C, for example, it can be 18°C, 20°C, 22°C, 25°C, 28°C, 30°C, 32°C, 35°C or 38°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range, and room temperature / normal temperature is further preferred.

[0034] Preferably, the pickling activation time is 20-40s, for example, it can be 22s, 25s, 28s, 30s, 32s, 35s or 38s, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0035] Preferably, the laser pulse energy of the laser etching is 10-20 μJ, for example, it can be 11 μJ, 12 μJ, 13 μJ, 14 μJ, 15 μJ, 16 μJ, 17 μJ, 18 μJ or 19 μJ, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0036] Preferably, the etching power of the laser etching is 5-20W, for example, it can be 6W, 8W, 10W, 12W, 14W, 15W, 16W, 18W or 19W, as well as specific point values ​​between the above point values. Due to limited space and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0037] Preferably, the etching speed of the laser etching is 50-650 mm / s, for example, it can be 80 mm / s, 100 mm / s, 150 mm / s, 200 mm / s, 250 mm / s, 300 mm / s, 350 mm / s, 400 mm / s, 450 mm / s, 500 mm / s, 550 mm / s, 600 mm / s or 620 mm / s, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0038] Preferably, the laser etching is performed 2-8 times, for example, 2 times, 3 times, 4 times, 5 times, 6 times, 7 times or 8 times.

[0039] Preferably, the etching spacing of the laser etching is 0.03-0.06mm, for example, it can be 0.032mm, 0.035mm, 0.038mm, 0.04mm, 0.042mm, 0.045mm, 0.048mm, 0.05mm, 0.052mm, 0.055mm or 0.058mm, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0040] Preferably, the laser repetition frequency of the laser etching is 1×10 6 -5×10 6 Hz, for example, it can be 1.5×10 6 Hz, 2×10 6 Hz, 2.5×10 6 Hz, 3×10 6 Hz, 3.5×10 6 Hz, 4×10 6 Hz, 4.5×10 6 Hz, 5×10 6 Hz or 5.5×10 6 Hz, and specific point values ​​between the above point values. Due to space limitations and for the sake of brevity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0041] As a preferred technical solution of the present invention, by adjusting the parameters of laser etching, a periodic micrometer-level structure with multi-level scales is formed on the surface of the metal substrate (stainless steel plate).

[0042] Preferably, the surface of the template comprises an array of pyramidal structures.

[0043] Preferably, the cone structure array includes a triangular cone array and / or a triangular cone array.

[0044] Preferably, the width of the conical structure is 50-300 μm, for example, it can be 60 μm, 80 μm, 100 μm, 120 μm, 150 μm, 180 μm, 200 μm, 220 μm, 250 μm or 280 μm, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0045] Preferably, the height of the conical structure is 10-300 μm, for example, it can be 20 μm, 50 μm, 80 μm, 100 μm, 120 μm, 150 μm, 180 μm, 200 μm, 220 μm, 250 μm or 280 μm, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0046] It should be noted that, in the direction perpendicular to the metal substrate, the cross-section of the conical structure is a triangle, and the width of the conical structure can be understood as the length of the base of the triangle; the height of the conical structure can be understood as the height of the triangle.

[0047] Preferably, the epoxy coating comprises a combination of epoxy resin and a curing agent.

[0048] In the present invention, the type of epoxy resin in the epoxy coating is not particularly limited, and conventional epoxy resins are applicable to the present invention. For example, the epoxy resin may be E51 epoxy resin.

[0049] Preferably, the curing agent in the epoxy coating includes any one of an amine curing agent, a phenolic curing agent, a phenolic amine curing agent, and an anhydride curing agent, or a combination of at least two of them.

[0050] Preferably, the mass ratio of epoxy resin to curing agent in the epoxy coating is 1:(0.1-0.8), for example, it can be 1:0.15, 1:0.2, 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45, 1:0.5, 1:0.55, 1:0.6, 1:0.65, 1:0.7 or 1:0.75, etc.

[0051] Preferably, the epoxy coating further includes a solvent, so that the epoxy coating reaches a viscosity suitable for use, so as to facilitate the coating of the epoxy coating, etc. In the subsequent drying step, the solvent in the epoxy coating will be partially or completely volatilized.

[0052] Preferably, the coating thickness of the epoxy coating is 40-60 μm, for example, it can be 42 μm, 45 μm, 48 μm, 50 μm, 52 μm, 55 μm or 58 μm, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0053] Preferably, the first drying temperature is 20-60°C, for example, it can be 22°C, 25°C, 28°C, 30°C, 32°C, 35°C, 38°C, 40°C, 42°C, 45°C, 48°C, 50°C, 52°C, 55°C or 58°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0054] Preferably, the first drying time is 0.5-12 h, for example, it can be 0.8 h, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 6.5 h, 7 h, 8 h, 9 h, 10 h, 11 h or 11.5 h, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0055] In the present invention, the type of epoxy resin in the photothermal hydrophobic coating is not particularly limited, and conventional epoxy resins are applicable to the present invention. Exemplarily, the epoxy resin may be E51 epoxy resin.

[0056] Preferably, the curing agent in the photothermal hydrophobic coating includes any one of an amine curing agent, a phenolic curing agent, a phenolic amine curing agent, and an anhydride curing agent, or a combination of at least two thereof, and an amine curing agent and / or a phenolic amine curing agent are further preferred.

[0057] Exemplarily, the amine curing agent includes any one of triethylenetetramine, diethylenetriamine, and dicyandiamide, or a combination of at least two thereof.

[0058] Exemplarily, the phenolic curing agent includes a phenolic resin, such as any one of a phenolic phenolic resin, a bisphenol A phenolic resin, a linear phenolic resin, and an o-cresol phenolic resin, or a combination of at least two thereof.

[0059] Preferably, the mass ratio of epoxy resin to curing agent in the photothermal hydrophobic coating is 1:(0.1-0.8), for example, it can be 1:0.15, 1:0.2, 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45, 1:0.5, 1:0.55, 1:0.6, 1:0.65, 1:0.7 or 1:0.75, etc.

[0060] As a preferred technical solution of the present invention, the photothermal filler is a carbon-based photothermal filler. The natural black carbon-based photothermal filler has broadband light absorption and contains a large amount of conjugated structures, thus having an excellent photothermal conversion effect.

[0061] Preferably, the photothermal filler includes any one of graphite, graphene, and graphene oxide, or a combination of at least two of them, and graphite is more preferred.

[0062] As a preferred technical solution of the present invention, the photothermal filler includes graphite, whose p orbitals on carbon atoms in the same plane can overlap with each other to form delocalized π bond electrons, which are easily excited, thereby having excellent photothermal conversion performance, while being low in cost and easy to plan for application.

[0063] Preferably, the mass ratio of epoxy resin to photothermal filler in the photothermal hydrophobic coating is 1:(0.01-0.4), for example, it can be 1:0.02, 1:0.05, 1:0.08, 1:0.1, 1:0.12, 1:0.15, 1:0.18, 1:0.2, 1:0.22, 1:0.25, 1:0.28, 1:0.3, 1:0.32, 1:0.35 or 1:0.38, etc.

[0064] Preferably, the fluorine-containing silane coupling agent includes any one of heptadecafluorodecyltriethoxysilane, heptadecafluorodecyltrimethoxysilane, tridecafluorooctyltrimethoxysilane and tridecafluorooctyltriethoxysilane, or a combination of at least two thereof.

[0065] Preferably, the mass ratio of epoxy resin to fluorine-containing silane coupling agent in the photothermal hydrophobic coating is 1:(0.001-0.2), for example, it can be 1:0.002, 1:0.005, 1:0.008, 1:0.01, 1:0.02, 1:0.05, 1:0.08, 1:0.1, 1:0.12, 1:0.15 or 1:0.18, etc.

[0066] Preferably, the photothermal hydrophobic coating also includes a solvent and / or a defoaming agent.

[0067] Preferably, the solvent in the photothermal hydrophobic coating includes any one of ketone solvents, alcohol solvents, ether solvents, aromatic hydrocarbon solvents, and ester solvents, or a combination of at least two of them.

[0068] Preferably, the solvent in the photothermal hydrophobic coating includes any one of acetone, butanone, cyclohexanone, methanol, and ethanol, or a combination of at least two of them.

[0069] Preferably, the mass ratio of epoxy resin to solvent in the photothermal hydrophobic coating is 1:(0.1-5), for example, it can be 1:0.2, 1:0.5, 1:0.8, 1:1, 1:1.2, 1:1.5, 1:1.8, 1:2, 1:2.2, 1:2.5, 1:2.8, 1:3, 1:3.2, 1:3.5, 1:3.8, 1:4, 1:4.2, 1:4.5 or 1:4.8, etc.

[0070] Preferably, the mass ratio of the defoamer to the curing agent in the photothermal hydrophobic coating is (0.01-1):100, for example, it can be 0.02:100, 0.05:100, 0.08:100, 0.1:100, 0.2:100, 0.3:100, 0.4:100, 0.5:100, 0.6:100, 0.7:100, 0.8:100 or 0.9:100, etc.

[0071] Preferably, the preparation method of the photothermal hydrophobic coating comprises: uniformly mixing epoxy resin, solvent, curing agent, photothermal filler, fluorine-containing silane coupling agent and optionally a defoaming agent to obtain the photothermal hydrophobic coating.

[0072] Further preferably, the preparation method of the photothermal hydrophobic coating includes: mixing and evenly dispersing an epoxy resin, a photothermal filler, a curing agent and a solvent to obtain a glue solution; and performing a second mixing of the glue solution with a fluorine-containing silane coupling agent to obtain the photothermal hydrophobic coating.

[0073] Preferably, the dispersing method includes ultrasonic dispersion and / or stirring dispersion.

[0074] Preferably, the power of the ultrasonic dispersion is 500-800 W, for example, it can be 520 W, 550 W, 580 W, 600 W, 620 W, 650 W, 680 W, 700 W, 720 W, 750 W or 780 W, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0075] Preferably, the ultrasonic dispersion time is 10-40 min, for example, it can be 12 min, 15 min, 18 min, 20 min, 22 min, 25 min, 28 min, 30 min, 32 min, 35 min or 38 min, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0076] Preferably, the stirring and dispersing rotation speed is 600-1000r / min, for example, it can be 650r / min, 700r / min, 750r / min, 800r / min, 850r / min, 900r / min or 950r / min, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0077] Preferably, the stirring and dispersing time is 0.5-2h, for example, it can be 0.6h, 0.8h, 1h, 1.2h, 1.5h or 1.8h, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0078] Preferably, the stirring speed of the second mixing is 800-1000r / min, for example, it can be 820r / min, 850r / min, 880r / min, 900r / min, 920r / min, 950r / min or 980r / min, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0079] Preferably, the second mixing time is 0.5-3h, for example, it can be 0.6h, 0.8h, 1h, 1.2h, 1.5h, 1.8h, 2h, 2.2h, 2.5h or 2.8h, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0080] Preferably, the coating thickness of the photothermal hydrophobic coating is 50-100 μm, for example, it can be 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm or 95 μm, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0081] Preferably, the second drying temperature is 20-60°C, for example, it can be 22°C, 25°C, 28°C, 30°C, 32°C, 35°C, 38°C, 40°C, 42°C, 45°C, 48°C, 50°C, 52°C, 55°C or 58°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0082] Preferably, the second drying time is 1-12 h, for example, it can be 1.2 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 6.5 h, 7 h, 8 h, 9 h, 10 h, 11 h or 11.5 h, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0083] As a preferred technical solution of the present invention, the extrusion is carried out in a hot press.

[0084] Preferably, the extrusion pressure is 5-10 MPa, for example, it can be 5.5 MPa, 6 MPa, 6.5 MPa, 7 MPa, 7.5 MPa, 8 MPa, 8.5 MPa, 9 MPa or 9.5 MPa, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0085] Preferably, the extrusion temperature is 15-40°C, for example, it can be 18°C, 20°C, 22°C, 25°C, 28°C, 30°C, 32°C, 35°C or 38°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range, and room temperature / normal temperature is further preferred.

[0086] Preferably, the extrusion time is 1-60 min, for example, it can be 2 min, 5 min, 8 min, 10 min, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min or 55 min, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0087] Preferably, the temperature of the third drying is 30-100°C, for example, it can be 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C or 95°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0088] Preferably, the third drying time is 1-12 h, for example, it can be 1.2 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 6.5 h, 7 h, 8 h, 9 h, 10 h, 11 h or 11.5 h, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0089] In a preferred technical solution, the preparation method comprises the following steps:

[0090] Laser etching the metal substrate to obtain a template with a microstructure on the surface;

[0091] The parameters of the laser etching are as follows: laser pulse energy is 10-20 μJ, etching power is 5-20 W, etching speed is 50-650 mm / s, etching spacing is 0.03-0.06 mm, laser repetition frequency is 1×10 6 -5×10 6 Hz, the etching times are 2-8 times; the surface microstructure of the template comprises a cone structure array, the cone structure has a width of 50-300 μm and a height of 10-300 μm;

[0092] Applying epoxy coating on the substrate, drying at 20-60° C. for 0.5-12 hours, to obtain a first coating;

[0093] The epoxy coating comprises an epoxy resin and a curing agent in a mass ratio of 1:(0.1-0.8), and the coating thickness of the epoxy coating is 40-60 μm;

[0094] Applying a photothermal hydrophobic coating on the first coating, and drying at 20-60° C. for 1-12 hours to obtain a photothermal coating;

[0095] The photothermal hydrophobic coating comprises an epoxy resin, a curing agent, a photothermal filler, a fluorinated silane coupling agent, a solvent and optionally a defoaming agent, wherein the mass ratio of the epoxy resin, the curing agent, the photothermal filler, the fluorinated silane coupling agent and the solvent in the photothermal hydrophobic coating is 1:(0.1-0.8):(0.01-0.4):(0.001-0.2):(0.1-5); the coating thickness of the photothermal hydrophobic coating is 50-100 μm;

[0096] The template is arranged on the photothermal coating so that the microstructure on the surface of the template contacts the photothermal coating, and then extruded at 5-10 MPa for 1-60 min, the template is removed, and dried at 30-100° C. for 1-12 h to obtain the photothermal super-hydrophobic coating.

[0097] In a second aspect, the present invention provides a photothermal super-hydrophobic coating, which is prepared by the preparation method described in the first aspect.

[0098] Preferably, the water contact angle of the photothermal super-hydrophobic coating is ≥150°, and may be 151-155°; and / or the rolling angle of the photothermal super-hydrophobic coating is 5-6°.

[0099] In a third aspect, the present invention provides an application of the photothermal superhydrophobic coating as described in the second aspect in deicing materials or anti-icing materials.

[0100] Preferably, the photothermal superhydrophobic coating can be applied to bridge cables, aircraft, buildings, electrical appliances, mechanical equipment or electrical equipment.

[0101] Compared with the prior art, the present invention has the following beneficial effects:

[0102] (1) The preparation method provided by the present invention introduces micro-nano imprinting technology, and the template imprinting method can be used to realize large-scale preparation of super-hydrophobic surfaces with directional arranged micro-nano structures, which has the advantages of good repeatability, low cost, and high structural resolution. At the same time, the template with microstructure on the surface can be used repeatedly, which significantly reduces the processing cost, shortens the processing time, and improves the production efficiency, and has a broad prospect for planned application.

[0103] (2) In the preparation method provided by the present invention, through the design and mutual combination of micro-nano imprinting technology, specific materials, and preparation process, the obtained photothermal super-hydrophobic coating has a super-hydrophobic surface with directional micro-nano structures, and a gradient-distributed photothermal filler is formed in the coating, thereby achieving excellent active deicing and passive deicing effects based on super-hydrophobic properties and photothermal conversion performance, thereby improving light utilization and photothermal conversion efficiency; the photothermal super-hydrophobic coating has good stability and UV aging resistance, effectively inhibits yellowing, has a long service life, and has excellent anti-icing durability, and can achieve long-term, stable and reliable active deicing and passive deicing effects, which is of great significance to various fields such as bridge cables, aircraft deicing, anti-fouling, and wearables. BRIEF DESCRIPTION OF THE DRAWINGS

[0104] Figure 1 A schematic diagram of the structure of a preparation method provided in a specific embodiment;

[0105] Figure 2 This is a water contact angle test diagram of the photothermal super-hydrophobic coating provided in Example 1. DETAILED DESCRIPTION

[0106] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0107] In the present invention, the features defined as "first", "second", and "third" may explicitly or implicitly include one or more of the features, and are used to distinguish and describe the features, without distinction of order or importance. In the description of the present invention, unless otherwise specified, the meaning of "plurality" is two or more.

[0108] As used herein, the terms "comprises," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0109] "Optionally" or "either" means that the subsequently described matter or event can or cannot occur, and that the description includes instances where the event occurs and instances where it does not.

[0110] After research, the present invention found that the existing passive anti-icing effect is not ideal, the photothermal super-hydrophobic layer is easy to break, the photothermal conversion capacity is insufficient, it is easy to age in an ultraviolet environment, the service life is short, and there are still certain problems in large-scale use.

[0111] In order to solve the aforementioned technical problems, a method for preparing a photothermal super-hydrophobic coating provided by a specific embodiment of the present invention comprises the following steps:

[0112] Laser etching the metal substrate to obtain a template with a microstructure on the surface;

[0113] Applying epoxy coating on the substrate and first drying to obtain a first coating;

[0114] Applying a photothermal hydrophobic coating on the first coating, and drying the coating to obtain a photothermal coating; the photothermal hydrophobic coating comprises a combination of an epoxy resin, a curing agent, a photothermal filler and a fluorine-containing silane coupling agent;

[0115] The template is arranged on the photothermal coating so that the microstructure on the surface of the template contacts the photothermal coating, and then the photothermal super-hydrophobic coating is obtained through extrusion, template removal and third drying.

[0116] In a specific embodiment, the structural schematic diagram of the preparation method is as follows Figure 1 As shown, the surface microstructure of the template includes a conical structure array, the width of the conical structure is 50-300μm, the height is 10-300μm, and the template surface has a periodic multi-scale micron-scale structure, which can be transferred to the photothermal coating by micro-nano-imprinting, so as to prepare a super-hydrophobic surface of a directional arrangement of micro-nano structures on a large scale, and the surface super-hydrophobic property brings excellent passive deicing effect. At the same time, in the photothermal super-hydrophobic coating, the concentration of the photothermal filler increases successively from the substrate to the coating surface; because the application of the photothermal filler itself will bring more internal defects to the coating, the photothermal filler at the coating close to the substrate in the present invention is less, and the corresponding defects are less, and the bonding force with the substrate is better; gradually transition to the coating surface, due to the increase in the content of the photothermal filler, the photothermal performance of the coating can be enhanced, and based on the micro-nano-imprinting technology, a very rich inverted triangle structure is formed, which can greatly enhance the multiple scattering of light particles in the inverted triangle structure, and multiple utilization of light energy, converted into heat energy, improve the utilization rate of light energy, and achieve the purpose of active deicing. Furthermore, in the photothermal super-hydrophobic coating with a photothermal filler concentration gradient, due to the high content of photothermal fillers on its surface, the energy density of ultraviolet light is reduced in the process of converting light energy into thermal energy, which can play a role in improving aging resistance.

[0117] The following are several examples of the photothermal super-hydrophobic coating and its preparation method according to the present invention; in the following examples, the epoxy resin used is E51 epoxy resin; the curing agent is triethylenetetramine, phenolic amine curing agent (T31 curing agent); the photothermal filler is graphite (GP), the size is 50-200nm, purchased from excellent alloy powder; the fluorine-containing silane coupling agent is heptadecafluorodecyltriethoxysilane (PFDTES).

[0118] Example 1

[0119] A photothermal super-hydrophobic coating and a preparation method thereof, the preparation method comprising the following steps:

[0120] (1) Preparation of template:

[0121] The pretreated stainless steel plate was placed on the laser processing work platform, and the laser pulse energy was adjusted to 10 μJ, the etching power to 10 W, the etching speed to 300 mm / s, the etching times to 4 times, the etching spacing to 0.03 mm, and the laser repetition frequency to 2 × 10 6 Hz, under this parameter combination, a template with a periodic multi-scale, micron-scale structure with a cone structure array was prepared on the surface of the stainless steel plate. The width of the cone structure was 200 μm and the height was 100 μm.

[0122] (2) Preparation of epoxy coating:

[0123] 10 g of E51 epoxy resin, 3.5 g of T31 curing agent and 5 g of acetone were mixed and stirred to prepare an epoxy coating;

[0124] (3) Preparation of photothermal hydrophobic coating:

[0125] 1g of graphite (GP) was added to 10g of E51 epoxy resin, and then mixed according to the formula of epoxy resin, acetone, and triethylenetetramine in a mass ratio of 10:5:3.5, the ultrasonic power was 600W, and the ultrasonic was performed for 30min to fully disperse it, and mechanically stirred and mixed at 800r / min for 1h at room temperature to obtain a glue solution. 0.6mL of 17-fluorodecyltriethoxysilane (PFDTES) was added to the above-obtained glue solution under stirring conditions, and mechanically stirred at 1000r / min for 3h at room temperature to obtain a photothermal hydrophobic coating.

[0126] (4) Preparation of photothermal super-hydrophobic coating:

[0127] The epoxy coating is coated on the substrate with a coating thickness (wet film thickness) of 40 μm and dried at 50° C. for 1 h to obtain a first coating;

[0128] Apply a photothermal hydrophobic coating on the first coating with a coating thickness of 50 μm, and dry at 50° C. for 5 h to obtain a photothermal coating;

[0129] The template prepared in step (1) is arranged on the photothermal coating so that the microstructure on the surface of the template contacts the photothermal coating, and then extruded at 5 MPa at room temperature for 10 min, the template is removed, and dried at 60° C. for 12 h to obtain the photothermal super-hydrophobic coating.

[0130] Example 2

[0131] A photothermal super-hydrophobic coating and a preparation method thereof, the preparation method comprising the following steps:

[0132] (1) Preparation of template:

[0133] The pretreated stainless steel plate was placed on the laser processing work platform, and the laser pulse energy was adjusted to 20 μJ, the etching power to 20 W, the etching speed to 300 mm / s, the etching times to 4 times, the etching spacing to 0.03 mm, and the laser repetition frequency to 2×10 6 Hz, under this parameter combination, a template with a periodic multi-scale, micron-scale structure with a cone structure array was prepared on the surface of the stainless steel plate. The width of the cone structure was 200 μm and the height was 100 μm.

[0134] (2) Preparation of epoxy coating:

[0135] 10 g of E51 epoxy resin, 3.5 g of T31 curing agent and 5 g of acetone were mixed and stirred to prepare an epoxy coating;

[0136] (3) Preparation of photothermal hydrophobic coating:

[0137] 2g of graphite (GP) was added to 15g of E51 epoxy resin, and then mixed according to the formula of epoxy resin, acetone, and triethylenetetramine in a mass ratio of 10:5:3.5, with an ultrasonic power of 800W, ultrasonic for 30min, and fully dispersed, and mechanically stirred and mixed at 1000r / min for 1h at room temperature to obtain a glue solution. 1mL of PFDTES was added to the above-obtained glue solution under stirring conditions, and mechanically stirred continuously at 1000r / min for 3h at room temperature to obtain a photothermal hydrophobic coating.

[0138] (4) Preparation of photothermal super-hydrophobic coating:

[0139] The epoxy coating is coated on the substrate with a coating thickness of 50 μm and dried at 50° C. for 1 h to obtain a first coating;

[0140] Apply a photothermal hydrophobic coating on the first coating to a thickness of 100 μm, and dry at 50° C. for 5 h to obtain a photothermal coating;

[0141] The template prepared in step (1) is placed on the photothermal coating so that the microstructure on the surface of the template contacts the photothermal coating, and then extruded at room temperature for 30 min at 10 MPa, the template is removed, and dried at 60° C. for 12 h to obtain the photothermal super-hydrophobic coating.

[0142] Example 3

[0143] (1) Preparation of template:

[0144] The pretreated stainless steel plate was placed on the laser processing work platform, and the laser pulse energy was adjusted to 20 μJ, the etching power to 10 W, the etching speed to 300 mm / s, the etching times to 8 times, the etching spacing to 0.06 mm, and the laser repetition frequency to 5 × 10 6 Hz, under this parameter combination, a template with a periodic multi-scale, micron-scale structure with a cone structure array was prepared on the surface of the stainless steel plate. The width of the cone structure was 100 μm and the height was 200 μm.

[0145] (2) Preparation of epoxy coating:

[0146] 10 g of E51 epoxy resin, 3.5 g of T31 curing agent and 5 g of acetone were mixed and stirred to prepare an epoxy coating;

[0147] (3) Preparation of photothermal hydrophobic coating:

[0148] 1.5 g of graphite (GP) was added to 20 g of E51 epoxy resin, and then mixed according to the formula of epoxy resin, acetone, and triethylenetetramine in a mass ratio of 10:5:3.5, with an ultrasonic power of 600 W, ultrasonic for 30 min, to fully disperse it, and mechanically stirred and mixed at 800 r / min for 1 h at room temperature to obtain a glue solution. 1 mL of PFDTES was added to the above-obtained glue solution under stirring conditions, and mechanically stirred continuously at 1000 r / min for 2 h at room temperature to obtain a photothermal hydrophobic coating.

[0149] (4) Preparation of photothermal super-hydrophobic coating:

[0150] The epoxy coating is coated on the substrate with a coating thickness of 40 μm and dried at 50° C. for 1.5 h to obtain a first coating;

[0151] Apply a photothermal hydrophobic coating on the first coating with a coating thickness of 80 μm, and dry at 50° C. for 5 h to obtain a photothermal coating;

[0152] The template prepared in step (1) is arranged on the photothermal coating so that the microstructure on the surface of the template contacts the photothermal coating, and then extruded at 5 MPa at room temperature for 10 min, the template is removed, and dried at 60° C. for 12 h to obtain the photothermal super-hydrophobic coating.

[0153] Comparative Example 1

[0154] A photothermal super-hydrophobic coating and a preparation method thereof, which differs from Example 1 only in that nanoimprinting is not performed, that is, a first coating and a photothermal coating are sequentially formed on a substrate by the same method as Example 1, and then dried at 60° C. for 12 hours to obtain the photothermal super-hydrophobic coating.

[0155] Comparative Example 2

[0156] A hydrophobic coating and a preparation method thereof, which differs from Example 1 only in that no graphite is added to the photothermal hydrophobic coating, and the components, amounts, preparation steps and process parameters of other materials are the same as those in Example 2 to obtain a hydrophobic coating.

[0157] Comparative Example 3

[0158] A photothermal super-hydrophobic coating and a preparation method thereof, which differs from Example 1 only in that no first coating is provided, that is, the photothermal hydrophobic coating is directly brushed on the substrate, the coating thickness is 50 μm, and the components, amounts, preparation steps and process parameters of other materials are the same as those in Example 1, to obtain a photothermal super-hydrophobic coating.

[0159] The following performance tests were performed on the photothermal super-hydrophobic coatings provided in Examples 1-3 and Comparative Examples 1-3:

[0160] (1) Photothermal conversion test

[0161] The photothermal super-hydrophobic coatings to be tested were placed under a irradiation intensity of 200 mW / cm 2 , under the condition of an ambient temperature of 35°C, the surface temperature of the coating after irradiation for different times was recorded, wherein the test data of Example 1 and Comparative Example 1 are shown in Table 1:

[0162] Table 1

[0163]

[0164] (2) Water contact angle and rolling angle test

[0165] The water contact angle on the surface of the photothermal super-hydrophobic coating was tested using a contact angle meter. The water contact angle test diagram of the photothermal super-hydrophobic coating provided in Example 1 is as follows: Figure 2 As shown in FIG. 2 , the water contact angle is 152° and the sliding angle is 6°; the test results of other embodiments and comparative examples are shown in Table 2.

[0166] (3) Aging resistance: The samples were placed in a high and low temperature UV aging test chamber. The test conditions were: irradiation intensity 0.6W / cm 2 , temperature 60℃; test the water contact angle of the sample every half an hour, stop the experiment when the contact angle is less than 150°, and record the placement time of the sample in the high and low temperature UV aging test box; the longer the time, the better the aging resistance; the test results are shown in Table 2.

[0167] Table 2

[0168]

[0169]

[0170] According to the performance data in Table 1 and Table 2, the photothermal super-hydrophobic coating obtained by the preparation method provided by the present invention heats up rapidly under illumination conditions, realizes efficient photothermal conversion, and has higher light utilization and photothermal conversion efficiency; at the same time, the water contact angle of the photothermal super-hydrophobic coating is 151-155°, and the rolling angle is 5-6°, which has outstanding hydrophobicity; the super-hydrophobic property of the photothermal super-hydrophobic coating can be maintained for ≥24h in the ultraviolet aging test, and has excellent aging resistance.

[0171] Comparative Example 1 does not have a directional arrangement of micro-nano structures, and its surface does not have super-hydrophobic properties, and the light utilization rate and photothermal conversion efficiency are also obviously insufficient. Comparative Example 2 does not contain photothermal filler graphite, and although it has super-hydrophobic properties, it cannot achieve photothermal conversion.

[0172] Furthermore, the photothermal superhydrophobic coating provided in Examples 1-3 and Comparative Example 3 was subjected to a durability test, and the method was as follows: first, the contact angle and photothermal conversion effect of the sample to be tested were tested (as shown in Tables 1 and 2, that is, the initial value); then the sample to be tested was placed in a culture dish, covered with water, and placed in a cold source at -10°C for 1 hour, and then taken out and tested for the time required for melting, the photothermal conversion effect and the contact angle, and compared with the initial value; repeatedly frozen and tested multiple times to reflect the downward trend of the contact angle and the change in the photothermal conversion effect.

[0173] The photothermal superhydrophobic coatings provided in Examples 1-3 exhibited excellent superhydrophobic and photothermal conversion properties in multiple freezing and thawing tests, and had excellent anti-icing durability; while although Comparative Example 3 initially had superhydrophobic and photothermal conversion properties, since the first coating was not set, the photothermal coating was in direct contact with the substrate, resulting in a significant attenuation of the contact angle and photothermal conversion performance after several freezing events, and insufficient durability.

[0174] It can be seen that the present invention introduces micro-nano embossing technology to prepare a super-hydrophobic anti-icing surface with a directional arrangement of microstructures. The micro-nano indentations can be directional, the surface roughness is uniform, there is no super-hydrophobic failure texture, and the coating with a photothermal filler concentration gradient can enhance the bonding strength between the coating and the substrate, and the inverted triangle microstructure can also use the energy of light particles multiple times. In summary, the present invention constructs a micro-convex structure on the surface of a coating with a photothermal filler (graphite) concentration gradient through micro-nano embossing technology to achieve the purpose of super-hydrophobic passive anti-icing; at the same time, graphite has a large number of conjugated structures, which have excellent light absorption and photothermal conversion properties. This photothermal active anti-icing technology is combined with super-hydrophobic passive anti-icing technology to produce a more excellent and durable and stable anti-icing effect, providing a new and efficient deicing method. In addition, the template imprinting method can realize the large-scale preparation of super-hydrophobic surfaces with directional arrangement of micro-nano structures, which has the advantages of good repeatability, low cost and high structural resolution, and has the potential for promotion and application, and has good practical application value.

[0175] The applicant declares that the present invention illustrates the photothermal super-hydrophobic coating of the present invention and its preparation method and application by the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. It should be clear to those skilled in the art that any improvement of the present invention, the equivalent replacement of the raw materials selected by the present invention, the addition of auxiliary components, the selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a photothermal super-hydrophobic coating, characterized in that: The preparation method comprises the following steps: Laser etching the metal substrate to obtain a template with a microstructure on the surface; Applying epoxy coating on the substrate and first drying to obtain a first coating; Applying a photothermal hydrophobic coating on the first coating, and drying the coating to obtain a photothermal coating; The photothermal hydrophobic coating comprises a combination of epoxy resin, curing agent, photothermal filler and fluorine-containing silane coupling agent; The template is arranged on the photothermal coating so that the microstructure on the surface of the template contacts the photothermal coating, and then the photothermal super-hydrophobic coating is obtained through extrusion, template removal and third drying.

2. The preparation method according to claim 1, characterized in that: The laser pulse energy of the laser etching is 10-20 μJ; Preferably, the etching power of the laser etching is 5-20W; Preferably, the etching speed of the laser etching is 50-650 mm / s; Preferably, the laser etching is performed 2-8 times; Preferably, the etching spacing of the laser etching is 0.03-0.06 mm; Preferably, the laser repetition frequency of the laser etching is 1×10 6 -5×10 6 Hz.

3. The preparation method according to claim 1 or 2, characterized in that: The surface of the template includes an array of pyramidal structures; Preferably, the width of the tapered structure is 50-300 μm; Preferably, the height of the cone structure is 10-300 μm.

4. The preparation method according to any one of claims 1 to 3, characterized in that The epoxy coating comprises a combination of epoxy resin and a curing agent; Preferably, the mass ratio of epoxy resin to curing agent in the epoxy coating is 1:(0.1-0.8); Preferably, the coating thickness of the epoxy coating is 40-60 μm; Preferably, the first drying temperature is 20-60°C; Preferably, the first drying time is 0.5-12 hours.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The mass ratio of epoxy resin to curing agent in the photothermal hydrophobic coating is 1:(0.1-0.8); Preferably, the photothermal filler includes any one of graphite, graphene, and graphene oxide, or a combination of at least two thereof; Preferably, the mass ratio of epoxy resin to photothermal filler in the photothermal hydrophobic coating is 1:(0.01-0.4); Preferably, the fluorine-containing silane coupling agent includes any one of heptadecafluorodecyltriethoxysilane, heptadecafluorodecyltrimethoxysilane, tridecafluorooctyltrimethoxysilane, and tridecafluorooctyltriethoxysilane, or a combination of at least two thereof; Preferably, the mass ratio of epoxy resin to fluorine-containing silane coupling agent in the photothermal hydrophobic coating is 1:(0.001-0.2); Preferably, the photothermal hydrophobic coating further comprises a solvent and / or a defoaming agent; Preferably, the mass ratio of epoxy resin to solvent in the photothermal hydrophobic coating is 1:(0.1-5); Preferably, the mass ratio of the defoamer to the curing agent in the photothermal hydrophobic coating is (0.01-1):100; Preferably, the preparation method of the photothermal hydrophobic coating comprises: uniformly mixing an epoxy resin, a solvent, a curing agent, a photothermal filler, a fluorine-containing silane coupling agent and optionally a defoaming agent to obtain the photothermal hydrophobic coating; Further preferably, the preparation method of the photothermal hydrophobic coating comprises: mixing and evenly dispersing an epoxy resin, a photothermal filler and a solvent to obtain a glue solution; performing a second mixing of the glue solution with a fluorinated silane coupling agent, and then performing a third mixing with a curing agent and optionally a defoaming agent to obtain the photothermal hydrophobic coating; Preferably, the dispersion method includes ultrasonic dispersion and / or stirring dispersion; Preferably, the power of the ultrasonic dispersion is 500-800W, and the time is 10-40min; Preferably, the stirring and dispersing speed is 600-1000 r / min, and the time is 0.5-2 h; Preferably, the stirring speed of the second mixing is 800-1000 r / min, and the time is 0.5-3 h; Preferably, the third mixing time is 5-10 min.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The coating thickness of the photothermal hydrophobic coating is 50-100 μm; Preferably, the second drying temperature is 20-60°C; Preferably, the second drying time is 1-12 hours.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The extrusion pressure is 5-10MPa; Preferably, the extrusion temperature is 15-40°C; Preferably, the extrusion time is 1-60min; Preferably, the temperature of the third drying is 30-100°C; Preferably, the third drying time is 1-12 hours.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: Laser etching the metal substrate to obtain a template with a microstructure on the surface; The parameters of the laser etching are as follows: laser pulse energy is 10-20 μJ, etching power is 5-20 W, etching speed is 50-650 mm / s, etching spacing is 0.03-0.06 mm, laser repetition frequency is 1×10 6 -5×10 6 Hz, the etching times are 2-8 times; the surface microstructure of the template comprises a cone structure array, the cone structure has a width of 50-300 μm and a height of 10-300 μm; Applying epoxy coating on the substrate, drying at 20-60° C. for 0.5-12 hours, to obtain a first coating; The epoxy coating comprises an epoxy resin and a curing agent in a mass ratio of 1:(0.1-0.8), and the coating thickness of the epoxy coating is 40-60 μm; Applying a photothermal hydrophobic coating on the first coating, and drying at 20-60° C. for 1-12 hours to obtain a photothermal coating; The photothermal hydrophobic coating comprises an epoxy resin, a curing agent, a photothermal filler, a fluorinated silane coupling agent, a solvent and optionally a defoaming agent, wherein the mass ratio of the epoxy resin, the curing agent, the photothermal filler, the fluorinated silane coupling agent and the solvent in the photothermal hydrophobic coating is 1:(0.1-0.8):(0.01-0.4):(0.001-0.2):(0.1-5); the coating thickness of the photothermal hydrophobic coating is 50-100 μm; The template is arranged on the photothermal coating so that the microstructure on the surface of the template contacts the photothermal coating, and then extruded at 5-10 MPa for 1-60 min, the template is removed, and dried at 30-100° C. for 1-12 h to obtain the photothermal super-hydrophobic coating.

9. A photothermal super-hydrophobic coating, characterized in that: The photothermal super-hydrophobic coating is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the photothermal super-hydrophobic coating according to claim 9 in deicing materials or anti-icing materials.

Citation Information

Patent Citations

  • Preparation method of active photo-thermal deicing coating with super-hydrophobic performance

    CN111073450A

  • Anti-icing and deicing coating layer with photo-thermal and self-cleaning performance and preparation method thereof

    CN113667400A

  • Transparent super-hydrophobic deicing coating as well as preparation method and application thereof

    CN116333592A

Cited By

  • Method for testing fatigue life of static sealing element in high-pressure and low-temperature environment

    CN119738282A

  • A method for testing the fatigue life of static seals under high pressure and low temperature conditions

    CN119738282B