Cold heading die and process for short and thick rod bolt

Through a multi-station cold heading machine, the diameter and shape of the rod material are gradually processed, the mold is controlled, and the four-sequence molding is designed reasonably, which solves the problem of the cold heading mold of short and thick rod bolts that is easy to damage, extends the mold life and improves the Molding quality.

CN119076884AActive Publication Date: 2024-12-06CHONGQING STANDARD FASTNERS IND CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411461457.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-12-06
Estimated Expiration
2044-10-18

AI Technical Summary

Technical Problem

The cold heading mold of the medium and medium-sized rod bolts in the prior art is subject to a large force, easy to damage, and has a short service life.

Method used

The rod material is gradually processed by a multi-station cold heading machine. Through one-sequence to four-sequence process steps, the diameter and shape of the rod material are deformed, so as to reduce the force of the mold, avoid excessive deformation and pressure concentration, and design a four-sequence mold lowering. To ensure molding quality and mold service life.

Benefits of technology

It effectively reduces the force of the mold, extends the service life of the mold, avoids mold damage caused by excessive upsetting pressure required for large deformation, and improves the cold heading forming quality of short and thick rod bolts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076884A_ABST
    Figure CN119076884A_ABST
Patent Text Reader

Abstract

The invention relates to the field of new energy automobile part production, and discloses a short and thick rod bolt cold heading die and process, through the improvement of the process and the die, one end of a rod material is shrunk, the other end of the rod material is upset into a conical surface structure in the first procedure, a thin rod is kept not stressed in the second procedure, and the conical surface structure is further upset in the third procedure, and then the thin rod is kept not stressed in the third procedure. Further upsetting the conical surface structure to form a hexagonal head initial blank, upsetting the conical surface structure into a step thick rod in the fourth procedure, and upsetting and forming the thin rod and the hexagonal head. A short-thick-rod bolt product with a step thick rod in the middle section can be directly formed through the cold heading process, and the problems that in the prior art, a short-thick-rod bolt cold heading die is large in stress and prone to damage, and the service life of the die is short can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of new energy automobile parts production, and in particular to a short thick rod bolt cold heading die and process. Background Art

[0002] New energy vehicles represent the future development direction of the automotive industry. They not only help reduce environmental pollution and improve energy efficiency, but also bring a more economical and smarter driving experience. With the continuous advancement of technology and the continued support of policies, the market share of new energy vehicles will continue to grow and become one of the mainstream means of transportation. A short thick rod bolt is required in scenarios such as battery packs, motors, reducers, suspension systems, transmission systems and body connections in new energy vehicles.

[0003] This short thick rod bolt has a disc-mounted head formed by a pressure plate at one end, a cylindrical thick rod with a larger diameter at the root of the other end, a shorter thick rod, and a cylindrical thin rod with a smaller diameter at the tail. Finally, threads are processed on the thin rod at the tail. In the prior art, during the cold forging process of the cover bolt, the rod at one end is first shrunk to form a thin rod portion, and the other end is upset to form a stepped thick rod. Then, the thin rod portion and the stepped thick rod portion are gradually upset to the final size in the second, third, and fourth sequences. The rod shrinking process of the thick rod portion and the thin rod portion and the pressure plate of the head are all formed at one time in the fourth sequence, and a step change is required in the radial structure of the mold. The combination of these three factors results in the mold being subjected to greater force, being easily damaged, and having a short service life. Summary of the invention

[0004] The present invention aims to provide a cold heading die for short thick shank bolts, so as to solve the problems in the prior art that the die is subjected to large force and is easily damaged, and the service life of the die is short, which exist in the cold heading process of short thick shank bolts.

[0005] To achieve the above object, the present invention adopts the following technical solution: a short thick rod bolt cold heading process, comprising the following steps:

[0006] A. Cutting: Cut the coiled steel into rods of a certain length, the diameter of which is 1.15 times the outer diameter of the thin rod of the short thick rod bolt;

[0007] B. In the first order, the lower end of the rod is shrunk to 0.9 times the outer diameter of the thin rod of the short thick rod bolt on the multi-station cold heading machine, and the middle section of the rod is upset to form a frustum. The minor diameter of the frustum is the same as the diameter of the lower end, the major diameter of the frustum is 0.94 times the outer diameter of the thick rod of the short thick rod bolt step, and the height of the frustum is 1.42 times the length of the thick rod of the short thick rod bolt step. The upper end of the rod is upset to form a frustum;

[0008] C. Second order: Use a multi-station cold upsetting machine to upset the top cone of the rod material to a cylinder with a spherical top surface, upset the middle cone to a height of 1.15 times the length of the thick rod of the short thick rod bolt step, upset the middle cone to a small diameter of 0.94 times the outer diameter of the thick rod of the short thick rod bolt step, upset the middle cone to a large diameter of 0.97 times the outer diameter of the thick rod of the short thick rod bolt step, and keep the diameter of the lower end of the rod material unchanged;

[0009] D. Three steps: use a multi-station cold upsetting machine to upset the cylindrical body at the upper end of the rod into a hexagonal head, form a pressure plate at the root of the hexagonal head, form a chamfer between the pressure plate and the middle section of the rod, upset the middle section of the rod to a small diameter of 0.96 times the outer diameter of the thick rod of the short thick rod bolt step, upset the middle section of the rod to a large diameter of 0.98 times the outer diameter of the thick rod of the short thick rod bolt step, and form a chamfer between the small diameter end of the middle section of the rod and the lower end of the rod;

[0010] E. Fourth step: Use a multi-station cold upsetting machine to further upset the hexagonal head at the upper end of the rod and form a hexagonal hole in the middle. Upset the pressure plate at the root of the hexagonal head to the forming size. Upset the middle section of the frustum to the forming size of an equal-diameter cylindrical step thick rod. Shrink the thin rod at the lower end to the forming size.

[0011] The principle and advantage of this scheme are as follows: in actual application, the diameter of the rod material is controlled during the blanking process, and then the upper end and the middle section of the rod material are upset into a truncated cone in the first sequence. In this way, the radial pressure on the middle section forming mold is small, and the lower end is shrunk. The blanking diameter of the lower end is close to the forming diameter, and the deformation amount in the rod shrinking process is small, so most of the deformation control can be completed in the first sequence; and then through the second sequence, the upper end of the rod material in the first sequence is further upset to form a cylinder, and the deformation amount is reduced in the subsequent hexagonal head forming process, which is easier to form. The truncated cone in the middle section is further upset and shortened but still maintains the taper. The deformation amount in a single sequence is small, the pressure on the mold is small, and the shrunk rod part at the lower end remains unchanged, that is, the shrunk rod part at the lower end is not subjected to force. In this way, the second sequence mold only bears radial deformation pressure at the upper end, and the mold as a whole is subjected to less force, which is not easy to cause damage to the second sequence mold. Then, the lower end of the shrink rod is kept free of stress through the third sequence, the upper hexagonal head is first upset and formed, and the middle section of the truncated cone is further upset and shortened while maintaining the taper. The deformation of the third sequence is relatively smaller, and it can be smoothly formed during the cold upsetting process, and it will not exert too much pressure on the mold, which can avoid damage to the mold. Finally, in the fourth sequence, the hexagonal head, pressure plate, step thick rod, and thin rod are upset and formed at one time. The forming deformation of the fourth sequence is greatly reduced compared with the existing technology, especially the step thick rod is formed through four deformation upsettings. During the process, the thin rod part is kept free of stress, which can effectively form under the premise of ensuring the service life of the mold, and can effectively avoid mold damage caused by excessive upsetting pressure required for large deformation.

[0012] The short thick rod bolt cold heading die is used to complete the short thick rod bolt cold heading process, including a four-sequence lower die, the four-sequence lower die includes a die sleeve, a rod reduction die is installed in the die sleeve, a C-shaped sleeve is arranged in the die sleeve at the upper end of the rod reduction die, a top die is arranged on the inner side of the C-shaped sleeve, a die sheet is arranged on the upper end of the top die, and a threaded sleeve is connected between the lower end of the rod reduction die and the die sleeve.

[0013] Preferably, as an improvement, the rod reduction mold, the top mold and the mold piece are all made of hard alloy.

[0014] Preferably, as an improvement, the C-type sleeve has a conical shape, the inner hole at the upper end of the mold sleeve is an inner tapered hole matching the shape of the C-type sleeve, and the C-type sleeve is pressed into the inner tapered hole by the threaded sleeve and the rod shrinking mold.

[0015] The principle and advantages of this scheme are as follows: in actual application, the four-sequence is the main forming process, the die sleeve in the four-sequence mold serves as an external support, the rod reduction mold, the top mold and the mold cavity inside the mold piece constitute the forming cavity of the short thick rod bolt, the rod reduction mold is used to form the thin rod at the lower end, the top mold and the mold piece are used to form the stepped thick rod in the middle section and the hexagonal head and pressure plate at the upper end, and the C-type sleeve is used to fix and guide the rod material to ensure the correct position of the rod material during the cold heading process and the stable and reliable forming quality. The rod reduction mold, the top mold and the mold piece are pressed and fixed by the taper match between the C-type sleeve and the die sleeve and the threaded sleeve at the bottom to further ensure the forming quality of the short thick rod bolt. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a schematic diagram of the deformation of the rod material during the processing in Example 1 of the present invention.

[0017] Figure 2 It is a schematic structural diagram of the four-sequence lower mold in Example 2 of the present invention. DETAILED DESCRIPTION

[0018] The following is further described in detail through specific implementation methods:

[0019] The reference numerals in the drawings of the specification include: a mold sleeve 1, a C-shaped sleeve 2, a mold piece 3, a top mold 4, a rod shrinking mold 5, and a threaded sleeve 6.

[0020] Example 1, a short thick rod bolt cold heading process, combined with Figure 1 As shown, the following steps are included:

[0021] A. Cutting: Cut the coiled steel into rods of a certain length, the diameter of which is 1.15 times the outer diameter of the thin rod of the short thick rod bolt;

[0022] B. In the first order, the lower end of the rod is shrunk to 0.9 times the outer diameter of the thin rod of the short thick rod bolt on the multi-station cold heading machine, and the middle section of the rod is upset to form a frustum. The minor diameter of the frustum is the same as the diameter of the lower end, the major diameter of the frustum is 0.94 times the outer diameter of the thick rod of the short thick rod bolt step, and the height of the frustum is 1.42 times the length of the thick rod of the short thick rod bolt step. The upper end of the rod is upset to form a frustum;

[0023] C. Second order: Use a multi-station cold upsetting machine to upset the top cone of the rod material to a cylinder with a spherical top surface, upset the middle cone to a height of 1.15 times the length of the thick rod of the short thick rod bolt step, upset the middle cone to a small diameter of 0.94 times the outer diameter of the thick rod of the short thick rod bolt step, and upset the middle cone to a large diameter of 0.97 times the outer diameter of the thick rod of the short thick rod bolt step, keeping the diameter of the lower end of the rod material unchanged, and the lower end of the rod material is not subjected to force;

[0024] D. Three steps: use a multi-station cold upsetting machine to upset the cylindrical body at the upper end of the rod into a hexagonal head, form a pressure plate at the root of the hexagonal head, form a chamfer between the pressure plate and the middle section of the rod, upset the middle section of the rod to a small diameter of 0.96 times the outer diameter of the thick rod of the short thick rod bolt step, upset the middle section of the rod to a large diameter of 0.98 times the outer diameter of the thick rod of the short thick rod bolt step, form a chamfer between the small diameter end of the middle section of the rod and the lower end of the rod, keep the diameter of the lower end of the rod unchanged, and the lower end of the rod is not subjected to force;

[0025] E. Fourth step: Use a multi-station cold upsetting machine to further upset the hexagonal head at the upper end of the rod and form a hexagonal hole in the middle. Upset the pressure plate at the root of the hexagonal head to the forming size. Upset the middle section of the frustum to the forming size of an equal-diameter cylindrical step thick rod. Shrink the thin rod at the lower end to the forming size.

[0026] During the specific implementation process, the diameter of the rod material is controlled during the blanking process, and then the upper end and the middle section of the rod material are upset into a frustum in the first sequence. In this way, the radial pressure on the middle section of the forming mold is small, and the lower end is shrunk. The blanking diameter of the lower end is close to the forming diameter, and the deformation in the rod shrinking process is small, so most of the deformation control can be completed in the first sequence; then after the second sequence, the upper end of the rod material in the first sequence is continued to be upset to form a cylinder. In the subsequent hexagonal head forming process, the deformation is reduced and it is easier to form. The frustum in the middle section is further upset and shortened but still maintains the taper. The deformation in a single sequence is small, the pressure on the mold is small, and the shrinking part of the lower end remains unchanged, that is, the shrinking part of the lower end is not subjected to force. In this way, the second sequence mold only bears radial deformation pressure at the upper end, and the overall force on the mold is small, which is not easy to cause damage to the second sequence mold. Then, the lower end of the shrink rod is kept free of stress through the third sequence, the upper hexagonal head is first upset and formed, and the middle section of the truncated cone is further upset and shortened while maintaining the taper. The deformation of the third sequence is relatively smaller, and it can be smoothly formed during the cold upsetting process, and it will not exert too much pressure on the mold, which can avoid damage to the mold. Finally, in the fourth sequence, the hexagonal head, pressure plate, step thick rod, and thin rod are upset and formed at one time. The forming deformation of the fourth sequence is greatly reduced compared with the existing technology, especially the step thick rod is formed through four deformation upsettings. During the process, the thin rod part is kept free of stress, which can effectively form under the premise of ensuring the service life of the mold, and can effectively avoid mold damage caused by excessive upsetting pressure required for large deformation.

[0027] Embodiment 2, a cold heading die for short thick rod bolts, used to complete the cold heading process of short thick rod bolts, includes a first-order die, a second-order die, a third-order die and a fourth-order die, wherein the first-order die includes a first-order lower die, the first-order lower die includes a first-order rod reduction die, the die cavity of the first-order rod reduction die includes a tapered rod cavity and a straight rod cavity, the tapered rod cavity is used to form the truncated cone in the middle section of the rod material, and the straight rod cavity is used to complete the rod reduction at the lower end of the rod material. The second-order die includes a second-order lower die, the die cavity of the second-order lower die includes a second-order tapered rod cavity and a second-order straight rod cavity, the second-order tapered rod cavity is used to further upset the truncated cone in the middle section of the rod material, the second-order straight rod cavity has the same inner diameter as the straight rod cavity of the first-order lower die, and is used to keep the thin rod at the lower end of the rod material free of stress during the second-order cold heading process. The lower die of the third-order die is similar in structure to the second-order lower die, but there is a size change, so that the truncated cone in the middle section is further upset, and the thin rod at the lower end is kept free of stress through the straight rod cavity. The four-sequence mold includes a four-sequence upper mold and a four-sequence lower mold, such as Figure 2 As shown, the lower die of the fourth sequence includes a die sleeve 1, a rod shrinking die 5 is installed in the die sleeve 1, a C-type sleeve 2 is arranged in the die sleeve 1 at the upper end of the rod shrinking die 5, a top die 4 is arranged inside the C-type sleeve 2, a die sheet 3 is arranged at the upper end of the top die 4, and a threaded sleeve 6 is connected between the lower end of the rod shrinking die 5 and the die sleeve 1. The rod shrinking die 5, top die 4 and die sheet 3 of the fourth sequence are all made of cemented carbide. The C-type sleeve 2 is conical in shape, and the inner hole at the upper end of the die sleeve 1 is an inner tapered hole matching the shape of the C-type sleeve 2. The C-type sleeve 2 is pressed tightly in the inner tapered hole through the threaded sleeve 6 and the rod shrinking die 5.

[0028] During the specific implementation process, the traditional first-order mold directly forms a cone at the top of the rod material, then forms a cylindrical section in the middle section, and forms a thin rod at the lower end. Then, the second order upsets the top cone into a spherical cylinder, and the middle section of the cylinder is upset to become shorter. The third and fourth orders continue to perform the same structural upsetting. In this way, the middle section is always upset as a cylinder, and the middle section and the lower end of the rod material are always under stress, especially in the fourth order, when the deformation is large. In this way, the molds from the second to fourth orders are under great stress, especially at the transition between the middle section step thick rod and the lower end thin rod. The step area is under great and concentrated stress, which can easily cause damage to the mold. In the scheme of Embodiment 1 and Embodiment 2, in the first process, the lower end of the rod material is shrunk into a thin rod, and the middle section is upset into a truncated cone shape, so that the force on the mold between the truncated cone and the thin rod is small, and then the thin rod part is kept free of force in the second process, and the truncated cone in the middle section is continuously upset, so that the diameter of the truncated cone becomes larger and the length becomes shorter, and the pressure concentration is reduced by chamfering between the truncated cone and the thin rod, and then the third process adopts the same method as the second process, continues to keep the thin rod free of force, further upsets the middle section truncated cone and maintains the chamfer transition between the truncated cone and the thin rod, and completes the preliminary forming of the top hexagonal head, and after the third process The middle section of the frustum and the top hexagonal structure are close to the forming size. In the four-series process, the middle section of the frustum is directly upset into a step thick rod. After the three-series processing, the chamfered transition part of the frustum to the step thick rod is flattened to form a step surface during the four-series forming process. In this way, the force on the mold is more reasonable, and it is not easy to be damaged during the cold forging process. The service life of the mold is longer. Such a mold combination cooperates with the corresponding cold forging forming process to directly cold forge short thick rod bolts. The mold structure is reasonably designed, and it is not easy to be damaged during use. It can produce and process short thick rod bolts for a long time to meet production needs.

[0029] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A cold heading process for short thick rod bolts, characterized in that: The following steps are involved: A. Cutting: Cut the coiled steel into rods of a certain length, the diameter of which is 1.15 times the outer diameter of the thin rod of the short thick rod bolt; B. In the first order, the lower end of the rod is shrunk to 0.9 times the outer diameter of the thin rod of the short thick rod bolt on the multi-station cold heading machine, and the middle section of the rod is upset to form a frustum. The minor diameter of the frustum is the same as the diameter of the lower end, the major diameter of the frustum is 0.94 times the outer diameter of the thick rod of the short thick rod bolt step, and the height of the frustum is 1.42 times the length of the thick rod of the short thick rod bolt step. The upper end of the rod is upset to form a frustum; C. Second order: Use a multi-station cold upsetting machine to upset the top cone of the rod material to a cylinder with a spherical top surface, upset the middle cone to a height of 1.15 times the length of the thick rod of the short thick rod bolt step, upset the middle cone to a small diameter of 0.94 times the outer diameter of the thick rod of the short thick rod bolt step, upset the middle cone to a large diameter of 0.97 times the outer diameter of the thick rod of the short thick rod bolt step, and keep the diameter of the lower end of the rod material unchanged; D. Three steps: use a multi-station cold upsetting machine to upset the cylindrical body at the upper end of the rod into a hexagonal head, form a pressure plate at the root of the hexagonal head, form a chamfer between the pressure plate and the middle section of the rod, upset the middle section of the rod to a small diameter of 0.96 times the outer diameter of the thick rod of the short thick rod bolt step, upset the middle section of the rod to a large diameter of 0.98 times the outer diameter of the thick rod of the short thick rod bolt step, and form a chamfer between the small diameter end of the middle section of the rod and the lower end of the rod; E. Fourth step: Use a multi-station cold upsetting machine to further upset the hexagonal head at the upper end of the rod and form a hexagonal hole in the middle. Upset the pressure plate at the root of the hexagonal head to the forming size. Upset the middle section of the frustum to the forming size of an equal-diameter cylindrical step thick rod. Shrink the thin rod at the lower end to the forming size.

2. Short thick rod bolt cold heading die, characterized by: A cold heading process for short thick rod bolts for completing claim 1 comprises a four-sequence lower die, the four-sequence lower die comprises a die sleeve, a rod reduction die is installed in the die sleeve, a C-shaped sleeve is arranged in the die sleeve at the upper end of the rod reduction die, a top die is arranged on the inner side of the C-shaped sleeve, a die sheet is arranged at the upper end of the top die, and a threaded sleeve is connected between the lower end of the rod reduction die and the die sleeve.

3. The large chamfer cold heading forming die for stud bolts according to claim 2, characterized in that: The rod shrinking mold, top mold and mold piece are all made of hard alloy.

4. The large chamfer cold heading forming die for stud bolts according to claim 3, characterized in that: The C-type sleeve has a conical shape, and the inner hole at the upper end of the mold sleeve is an inner conical hole matching the shape of the C-type sleeve. The C-type sleeve is pressed tightly in the inner conical hole through the threaded sleeve and the rod shrinking mold.

Citation Information

Patent Citations

  • Machining method and machining mold assembly for hexagonal bolt

    CN105269246A

  • Bolt large chamfering cold heading die and process

    CN108787979A

  • Thick-rod hexagon-headed bolt cold heading process

    CN113500158A

  • Forming process of short half-tooth flange face hexagon bolt

    CN116078964A

  • Cold -heading equipment is used in processing of car bolt