Aluminum alloy laser ceramic / high-entropy alloy composite powder filling welding method

By using ceramic/high entropy alloy composite powder in aluminum alloy laser powder welding, the problem of reduced strength of aluminum alloy welding joints is solved, and the significant improvement of weld strength and improvement of welding forming is achieved.

CN119077129AActive Publication Date: 2024-12-06SOUTH CHINA UNIV OF TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411042003.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-12-06
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Due to the low absorption rate of aluminum alloy during laser welding, the weld area is significantly softened, and the strength of the weld joint is significantly lower than that of the base material. In the prior art, ceramic/high entropy alloy composite powder is not used for aluminum alloy laser powder filling welding.

Method used

Ceramic/high-entropy alloy composite powder is used as the filling material to prepare ceramic/high-entropy alloy composite powder through plasma spheroidization, and the aluminum alloy plate is surface treated and dried before welding. The laser powder filling welding process is used for welding. The synergistic effect of ceramic powder and high entropy alloy powder improves the strength of welded joints.

Benefits of technology

It significantly improves the strength of welds, reduces the formation of intermetallic compounds in welds, and adjusts the types and ratios of ceramic powder and high-entropy alloy powder, and is suitable for different aluminum alloy materials to obtain different reinforcement effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119077129A_ABST
    Figure CN119077129A_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum alloy laser ceramic / high-entropy alloy composite powder filling welding method, which belongs to the technical field of welding, and comprises the following steps: (1) composite powder preparation: ceramic powder and high-entropy alloy powder are subjected to plasma spheroidization according to a certain proportion to obtain ceramic / high-entropy alloy composite powder; (2) pretreatment of a welding sample: polishing the to-be-welded surface of the to-be-welded aluminum alloy plate and an area 25mm around a welding seam to remove an oxidation film, wiping the to-be-welded surface and the area 25mm around the welding seam by adopting a volatile organic solvent, and then putting the to-be-welded aluminum alloy plate into drying equipment to be dried; (3) the aluminum alloy plates in the step (2) are placed in a butt joint mode and fixed through a pressing plate, and a to-be-welded structure is formed; and (4) welding the to-be-welded structure in the step (3) by adopting a laser powder filling welding process. According to the method, the ceramic / high-entropy alloy composite powder is evenly distributed in the welding seam by means of the stirring effect of laser on the molten pool, the advantages of ceramic particle reinforcement and high-entropy alloy particle reinforcement are achieved, and the strength of a welding seam joint can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of welding, and in particular provides an aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method. Background Art

[0002] Aluminum alloy has become the preferred lightweight material for reducing the weight of the vehicle body and improving fuel efficiency in today's automotive industry, especially in the new energy vehicle industry, due to its advantages such as low density, excellent mechanical properties and corrosion resistance. In the production and manufacturing process of the vehicle body and parts, it is inevitable to consider the connection problem. Therefore, how to achieve efficient and high-quality connection of aluminum alloy is of great significance to vehicle body manufacturing. As an emerging welding technology, laser welding has received more and more attention in the field of aluminum alloy welding due to its advantages such as small welding deformation, small heat-affected zone and wide processing range. However, as a highly reflective material, aluminum alloy has a low absorption rate for laser. In addition, under the action of laser, the original fine structure and nano-precipitation phase in the parent material cannot be retained, resulting in obvious softening in the weld zone and significantly lower strength of the welded joint than that of the parent material.

[0003] Laser powder welding is to supplement the molten pool with metal or non-metal powder during welding. Compared with laser autogenous welding, the utilization rate is improved, the assembly precision requirement is lower, and it is convenient to adjust during welding; at the same time, the types of filler materials are rich, and the composition is easy to control to meet different application requirements; by adding effective ingredients, a more stable welding effect can be obtained, the weld formation is improved, the defects are suppressed, and the mechanical properties of the joint are improved.

[0004] At present, for aluminum alloy laser filling powder, single powder or its mixed powder is mostly used, such as Si powder, Cu powder, Zr powder, Mn powder, etc. and some ceramic particles. For example, Chinese patent (CN108723596A) relies on the stirring effect of laser on the molten pool to evenly distribute TiB2 particles in the weld, and the stability of ceramic particles during laser welding significantly improves the strength of the weld joint. High entropy alloys have excellent mechanical properties. Compared with ceramic materials, high entropy alloys have better wettability with aluminum matrix and higher interface bonding strength. At present, some scholars have tried to apply high entropy alloys to the field of welding. For example, Chinese patent (CN101554685A) discloses a high entropy alloy brazing material for welding copper and aluminum and its preparation method. However, at present, there is no report on the use of ceramic / high entropy alloy composite powder as filling powder for aluminum alloy laser filling powder welding. In view of the above analysis, this patent application proposes to use ceramic / high entropy alloy composite powder as filling material for aluminum alloy laser filling powder welding, relying on the synergistic effect of ceramic powder and high entropy alloy powder to improve the strength of the weld joint. Summary of the invention

[0005] In order to overcome the deficiencies in the prior art, the present invention provides an aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method.

[0006] The technical solution of the present invention is:

[0007] A method for welding aluminum alloy laser ceramic / high entropy alloy composite powder, comprising the following steps:

[0008] (1) Preparation of composite powder: Ceramic powder and high entropy alloy powder are spheroidized by plasma in a certain ratio to obtain ceramic / high entropy alloy composite powder;

[0009] (2) Pretreatment of welding samples: Grind the surface of the aluminum alloy plate to be welded and the 25mm area around the weld to remove the oxide film, wipe it clean with a volatile organic solvent, and then put it in a drying equipment for drying;

[0010] (3) placing the aluminum alloy plates obtained in step (2) in a butt-jointed manner and fixing them with a pressing plate to form a structure to be welded;

[0011] (4) The structure to be welded described in step (3) is welded using a laser powder filling welding process.

[0012] In the above method, in step (1), the ceramic powder includes TiB2, TiC, TiN, SiC, ZrO2, etc.; the high entropy alloy powder includes FeCoCrNi series, FeCoCrNiMn series, FeCoCrNiMo series, AlCoCrFeNi series, AlTiCrNiCu series, WTaMoNbV series, TiNbZrTa series, etc.

[0013] In the above method, in step (1), the mass fraction of the ceramic in the ceramic / high entropy alloy composite powder is between 1% and 50%, the mass fraction of the high entropy alloy is between 50% and 99%, and the sum of the two is equal to 1. The ceramic powder is flaky or other irregular shapes with a particle size of 0.05 to 1 μm, the high entropy alloy powder is spherical with a particle size of 1 to 100 μm, and the ceramic / high entropy alloy composite powder is spherical with a particle size of 1 to 100 μm.

[0014] In the above method, in step (2), the aluminum alloy includes cast aluminum alloys, such as Al-Si series, Al-Cu series, Al-Mg series, Al-Zn series; and also includes deformed aluminum alloys.

[0015] In the above method, in step (2), the thickness of the aluminum alloy to be welded is 1-6 mm.

[0016] In the above method, in step (2), when the thickness of the aluminum alloy to be welded is 1-3 mm, no groove is made; when the thickness is 4-6 mm, a groove is made, and the groove shapes include "I" shape, "V" shape, "Y" shape, etc.

[0017] In the above method, in step (2), the volatile organic solvent includes ethanol, acetone, etc.

[0018] In the above method, in step (2), the drying temperature is 60-80° C. and the drying time is 20-40 min.

[0019] In the above method, in step (4), the ceramic / high entropy alloy composite powder filling method includes a pre-set powder method and a synchronous powder feeding method, wherein the synchronous powder feeding method includes coaxial powder feeding and side-axis powder feeding.

[0020] In the above method, in step (4), high-purity argon gas with a mass concentration of not less than 99.99% is used for coaxial protection during welding, and the flow rate of the protective gas is 10-20 L / min.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The present invention adds ceramic / high entropy alloy composite powder to the aluminum alloy weld through a laser powder filling welding process, and relies on the dispersion strengthening of the composite powder to significantly improve the weld strength.

[0023] 2. The present invention adds ceramic / high entropy alloy composite powder into the aluminum alloy weld through a laser powder filling welding process, and relies on the hysteresis diffusion effect of the high entropy alloy to reduce the formation of intermetallic compounds in the weld.

[0024] 3. The present invention adjusts the types and proportions of different ceramic powders and high entropy alloy powders, and can be applied to different aluminum alloy materials to obtain different strengthening effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a schematic diagram of laser powder filling welding of aluminum alloy according to the present invention.

[0026] Figure 2 This is a macroscopic morphology of the weld in Example 1 of the present invention.

[0027] Figure 3 This is a macroscopic morphology of the weld of the comparative example of the present invention. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further described below in conjunction with specific embodiments, but is not limited thereto.

[0029] Example 1

[0030] This embodiment provides a 1 mm thick 6063 aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method, specifically comprising:

[0031] (1) Composite powder preparation: TiC ceramic powder with an average particle size of 0.5 μm and AlCoCrFeNi high entropy alloy powder with an average particle size of 15 to 53 μm were plasma spheroidized in a mass ratio of 10:90 to obtain ceramic / high entropy alloy composite powder.

[0032] (2) Pretreatment of welding samples: The surface of the 1 mm thick 6063 aluminum alloy plate to be welded and the 25 mm area around the weld were polished to remove the oxide film, without opening the groove, and wiped clean with anhydrous ethanol, and then placed in an 80 ° C drying equipment for 30 minutes for drying.

[0033] (3) The 6063 aluminum alloy plates of step (2) are placed in a butt joint and fixed by a pressing plate to form a structure to be welded.

[0034] (4) The structure to be welded in step (3) is welded by laser powder filling welding process, and the powder feeding method is coaxial powder feeding. The specific welding parameters are as follows: laser power is 1100W, welding speed is 30mm / s, defocusing amount is 0, powder feeding amount is 3.5g / min, and shielding gas flow rate is 10L / min.

[0035] The macroscopic morphology of the weld in this embodiment is as follows Figure 2 As shown, the weld surface is well formed without forming defects such as undercut and spatter. The tensile strength of the weld sample is 215.8MPa and the weld strength coefficient is 82.7%.

[0036] Example 2

[0037] This embodiment provides a 2 mm thick 2024 aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method, specifically comprising:

[0038] (1) Composite powder preparation: TiB2 ceramic powder with an average particle size of 0.1 μm and AlCoCrFeNi high entropy alloy powder with an average particle size of 15-53 μm were plasma spheroidized in a mass ratio of 30:70 to obtain ceramic / high entropy alloy composite powder.

[0039] (2) Pretreatment of welding samples: The surface of the 2 mm thick 2024 aluminum alloy plate to be welded and the 25 mm area around the weld were polished to remove the oxide film, without opening the groove, and wiped clean with anhydrous ethanol, and then placed in an 80 ° C drying equipment for 30 minutes for drying.

[0040] (3) The 2024 aluminum alloy plates of step (2) are placed in a butt joint and fixed by a pressing plate to form a structure to be welded.

[0041] (4) The structure to be welded in step (3) is welded by laser powder filling welding process, and the powder feeding method is coaxial powder feeding. The specific welding parameters are as follows: laser power is 1700W, welding speed is 30mm / s, defocusing amount is +1, powder feeding amount is 6g / min, and shielding gas flow rate is 12L / min.

[0042] The weld surface of this embodiment is well formed without forming defects such as undercut and spatter. The tensile strength of the weld sample is 335.4 MPa, and the weld strength coefficient is 72.9%.

[0043] Example 3

[0044] This embodiment provides a 4 mm thick ZL101 aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method, specifically comprising:

[0045] (1) Composite powder preparation: TiB2 ceramic powder with an average particle size of 0.8 μm and FeCoCrNi high entropy alloy powder with an average particle size of 15-53 μm were plasma spheroidized in a mass ratio of 20:80 to obtain ceramic / high entropy alloy composite powder.

[0046] (2) Pretreatment of welding samples: The surface of the 4 mm thick ZL101 aluminum alloy plate to be welded and the 25 mm area around the weld were ground to remove the oxide film, a "V"-shaped groove was opened, and it was wiped clean with acetone and then placed in an 80°C drying equipment for 30 minutes for drying.

[0047] (3) The ZL101 aluminum alloy plates of step (2) are placed in a butt joint and fixed by a pressing plate to form a structure to be welded.

[0048] (4) The structure to be welded in step (3) is welded by laser powder filling welding process, and the powder feeding method is side axis powder feeding. The specific welding parameters are as follows: laser power is 2800W, welding speed is 20mm / s, defocus is -1, powder feeding amount is 12g / min, and shielding gas flow rate is 15L / min.

[0049] The weld surface of this embodiment is well formed without forming defects such as undercut and spatter. The tensile strength of the weld sample is 230.4 MPa, and the weld strength coefficient is 78.1%.

[0050] Example 4

[0051] This embodiment provides a 6 mm thick 7075 aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method, specifically comprising:

[0052] (1) Composite powder preparation: ZrO2 ceramic powder with an average particle size of 0.6 μm and TiNbZrTa high entropy alloy powder with an average particle size of 1 to 25 μm were plasma spheroidized in a mass ratio of 50:50 to obtain ceramic / high entropy alloy composite powder.

[0053] (2) Pretreatment of welding specimens: The surface of the 6 mm thick 7075 aluminum alloy plate to be welded and the 25 mm area around the weld were polished to remove the oxide film, a "Y"-shaped groove was opened, and it was wiped clean with anhydrous ethanol, and then placed in an 80 ° C drying equipment for 30 minutes for drying.

[0054] (3) The 7075 aluminum alloy plates of step (2) are placed in a butt joint and fixed by a pressing plate to form a structure to be welded.

[0055] (4) The structure to be welded in step (3) is welded by laser powder filling welding process, and the powder feeding method is coaxial powder feeding. The specific welding parameters are as follows: laser power is 4300W, welding speed is 25mm / s, defocusing amount is -2, powder feeding amount is 15g / min, and shielding gas flow rate is 15L / min.

[0056] The weld surface of this embodiment is well formed without forming defects such as undercut and spatter. The tensile strength of the weld sample is 385.8 MPa, and the weld strength coefficient is 70.7%.

[0057] Example 5

[0058] This embodiment provides a 4 mm thick 5083 aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method, specifically comprising:

[0059] (1) Composite powder preparation: TiB2 ceramic powder with an average particle size of 0.5 μm and AlTiCrNiCu high entropy alloy powder with an average particle size of 15-53 μm were plasma spheroidized in a mass ratio of 40:60 to obtain ceramic / high entropy alloy composite powder.

[0060] (2) Pretreatment of welding specimens: The surface of the 4 mm thick 5083 aluminum alloy plate to be welded and the 25 mm area around the weld were ground to remove the oxide film, an "I" groove was opened, and it was wiped clean with anhydrous ethanol, and then placed in an 80 ° C drying equipment for 30 minutes for drying.

[0061] (3) The 5083 aluminum alloy plates of step (2) are placed in a butt joint and fixed by a pressing plate to form a structure to be welded.

[0062] (4) The structure to be welded in step (3) is welded by laser powder filling welding process, and the powder feeding method is coaxial powder feeding. The specific welding parameters are as follows: laser power is 3200W, welding speed is 25mm / s, defocusing amount is -1, powder feeding amount is 11g / min, and shielding gas flow rate is 15L / min.

[0063] The weld surface of this embodiment is well formed without forming defects such as undercut and spatter. The tensile strength of the weld sample is 297.6 MPa, and the weld strength coefficient is 86.3%.

[0064] Example 6

[0065] This embodiment provides a 3 mm thick 3003 aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method, specifically comprising:

[0066] (1) Composite powder preparation: TiC ceramic powder with an average particle size of 0.5 μm and FeCoCrNiMn high entropy alloy powder with an average particle size of 15 to 53 μm were plasma spheroidized in a mass ratio of 25:75 to obtain ceramic / high entropy alloy composite powder.

[0067] (2) Pretreatment of welding specimens: The surface of the 3 mm thick 3003 aluminum alloy plate to be welded and the 25 mm area around the weld were polished to remove the oxide film, without opening the groove, and wiped clean with anhydrous ethanol, and then placed in an 80 ° C drying equipment for 30 min.

[0068] (3) The 3003 aluminum alloy plates of step (2) are placed in a butt joint and fixed by a pressing plate to form a structure to be welded.

[0069] (4) The structure to be welded in step (3) is welded by laser powder filling welding process, and the powder feeding method is coaxial powder feeding. The specific welding parameters are as follows: laser power is 2600W, welding speed is 20mm / s, defocusing amount is 0, powder feeding amount is 10.5g / min, and shielding gas flow rate is 15L / min.

[0070] The weld surface of this embodiment is well formed without forming defects such as undercut and spatter. The tensile strength of the weld sample is 253 MPa, and the weld strength coefficient is 85%.

[0071] Example 7

[0072] This embodiment provides a 2.5 mm thick 6005A aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method, specifically comprising:

[0073] (1) Composite powder preparation: ZrO2 ceramic powder with an average particle size of 0.5 μm and TiNbZrTa high entropy alloy powder with an average particle size of 1 to 25 μm were plasma spheroidized in a mass ratio of 5:95 to obtain ceramic / high entropy alloy composite powder.

[0074] (2) Pretreatment of welding samples: The surface of the 2.5 mm thick 6005A aluminum alloy plate to be welded and the 25 mm area around the weld were polished to remove the oxide film, without opening the groove, and wiped clean with anhydrous ethanol, and then placed in an 80 ° C drying equipment for 30 minutes for drying.

[0075] (3) The 6005A aluminum alloy plates of step (2) are placed in a butt joint and fixed by a pressing plate to form a structure to be welded.

[0076] (4) The structure to be welded in step (3) is welded by laser powder filling welding process, and the powder feeding method is coaxial powder feeding. The specific welding parameters are as follows: laser power is 2400W, welding speed is 30mm / s, defocusing amount is 0, powder feeding amount is 9.8g / min, and shielding gas flow rate is 14L / min.

[0077] The weld surface of this embodiment is well formed without forming defects such as undercut and spatter. The tensile strength of the weld sample is 248.7 MPa, and the weld strength coefficient is 74.9%.

[0078] Example 8

[0079] This embodiment provides a 2 mm thick 6016 aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method, specifically comprising:

[0080] (1) Composite powder preparation: TiN ceramic powder with an average particle size of 0.5 μm and AlCoCrFeNi2.1 high entropy alloy powder with an average particle size of 1 to 25 μm were plasma spheroidized in a mass ratio of 15:85 to obtain ceramic / high entropy alloy composite powder.

[0081] (2) Pretreatment of welding samples: The surface of the 2 mm thick 6016 aluminum alloy plate to be welded and the 25 mm area around the weld were polished to remove the oxide film, without opening the groove, and wiped clean with anhydrous ethanol, and then placed in an 80 ° C drying equipment for 30 minutes for drying.

[0082] (3) The 6016 aluminum alloy plates of step (2) are placed in a butt joint and fixed by a pressing plate to form a structure to be welded.

[0083] (4) The structure to be welded in step (3) is welded by laser powder filling welding process, and the powder feeding method is coaxial powder feeding. The specific welding parameters are as follows: laser power is 1900W, welding speed is 35mm / s, defocusing amount is -1, powder feeding amount is 7.8g / min, and shielding gas flow rate is 12L / min.

[0084] The weld surface of this embodiment is well formed without forming defects such as undercut and spatter. The tensile strength of the weld sample is 183.4 MPa, and the weld strength coefficient is 78.4%.

[0085] Example 9

[0086] This embodiment provides a 2 mm thick ZL101 aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method, specifically comprising:

[0087] (1) Composite powder preparation: TiB2 ceramic powder with an average particle size of 0.5 μm and AlTiCrNiCu high entropy alloy powder with an average particle size of 15-53 μm were plasma spheroidized in a mass ratio of 1:99 to obtain ceramic / high entropy alloy composite powder.

[0088] (2) Pretreatment of welding samples: The surface of the 2 mm thick ZL101 aluminum alloy plate to be welded and the 25 mm area around the weld were polished to remove the oxide film, without opening the groove, and wiped clean with anhydrous ethanol, and then placed in an 80 ° C drying equipment for 30 min.

[0089] (3) The ZL101 aluminum alloy plates of step (2) are placed in a butt joint and fixed by a pressing plate to form a structure to be welded.

[0090] (4) The structure to be welded in step (3) is welded by laser powder filling welding process, and the powder feeding method is coaxial powder feeding. The specific welding parameters are as follows: laser power is 1800W, welding speed is 30mm / s, defocusing amount is -1, powder feeding amount is 6.2g / min, and shielding gas flow rate is 12L / min.

[0091] The weld surface of this embodiment is well formed without forming defects such as undercut and spatter. The tensile strength of the weld sample is 237.8 MPa, and the weld strength coefficient is 80.6%.

[0092] Comparative Example:

[0093] This comparative example provides a 1 mm thick 6063 aluminum alloy laser self-fusion welding method, specifically comprising:

[0094] (1) Pretreatment of welding specimens: The surface of the 1 mm thick 6063 aluminum alloy plate to be welded and the 25 mm area around the weld were polished to remove the oxide film, without opening the groove, and wiped clean with anhydrous ethanol, and then placed in an 80 ° C drying equipment for 30 min for drying.

[0095] (2) The 6063 aluminum alloy plates of step (2) are placed in a butt joint and fixed by a pressing plate to form a structure to be welded.

[0096] (3) The structure to be welded in step (2) is welded by laser autogenous welding process. The specific welding parameters are as follows: laser power is 950W, welding speed is 30mm / s, defocusing amount is 0, and shielding gas flow rate is 10L / min.

[0097] The macroscopic morphology of the weld in this comparative example is as follows Figure 3 As shown, the front side of the weld is slightly collapsed, the tensile strength of the welded sample is 188.7MPa, and the weld strength coefficient is 72.3%.

[0098] The above is only a specific implementation of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention are all covered by the protection scope of the present invention.

Claims

1. A method for welding aluminum alloy laser ceramic / high entropy alloy composite powder, characterized in that: The steps include: (1) Composite powder preparation: Ceramic powder and high entropy alloy powder are plasma spheroidized in a certain mass ratio to obtain ceramic / high entropy alloy composite powder; (2) Pretreatment of welding samples: Grind the surface of the aluminum alloy plate to be welded and the 25mm area around the weld to remove the oxide film, wipe it clean with a volatile organic solvent, and then put it in a drying equipment for drying; (3) placing the aluminum alloy plates obtained in step (2) in a butt-jointed manner and fixing them with a pressing plate to form a structure to be welded; (4) The structure to be welded described in step (3) is welded using a laser powder filling welding process.

2. According to claim 1, a method for welding aluminum alloy laser ceramic / high entropy alloy composite powder, characterized in that: In step (1), the ceramic powder includes TiB2, TiC, TiN, SiC or ZrO2; the high entropy alloy powder includes FeCoCrNi series, FeCoCrNiMn series, FeCoCrNiMo series, AlCoCrFeNi series, AlTiCrNiCu series, WTaMoNbV series or TiNbZrTa series.

3. According to claim 1, the aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method is characterized in that: In step (1), the mass fraction of ceramic in the ceramic / high entropy alloy composite powder is between 1% and 50%, the mass fraction of high entropy alloy is between 50% and 99%, and the sum of the two is equal to 1; the ceramic powder is flaky or other irregular shapes and has a particle size of 0.05 to 1 μm, the high entropy alloy powder is spherical and has a particle size of 1 to 100 μm, and the ceramic / high entropy alloy composite powder is spherical and has a particle size of 1 to 100 μm.

4. The aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method according to claim 1, characterized in that: In step (2), the aluminum alloy includes a cast aluminum alloy and a deformed aluminum alloy, and the cast aluminum alloy includes an Al-Si series, an Al-Cu series, an Al-Mg series or an Al-Zn series.

5. The aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method according to claim 1, characterized in that: In step (2), the thickness of the aluminum alloy to be welded is 1-6 mm.

6. The aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method according to claim 5, characterized in that: In step (2), when the thickness of the aluminum alloy to be welded is 1-3 mm, no groove is made; when the thickness is 4-6 mm, a groove is made, and the groove shape includes "I" shape, "V" shape or "Y" shape.

7. The aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method according to claim 1, characterized in that: In step (2), the volatile organic solvent includes ethanol or acetone.

8. The aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method according to claim 1, characterized in that: In step (2), the drying temperature is 60-80° C. and the drying time is 20-40 min.

9. The aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method according to claim 1, characterized in that: In step (4), the ceramic / high entropy alloy composite powder filling method includes a pre-set powder method and a synchronous powder feeding method, wherein the synchronous powder feeding method includes coaxial powder feeding and side-axis powder feeding.

10. The aluminum alloy laser ceramic / high entropy alloy composite powder filling welding method according to claim 1, characterized in that: In step (4), high-purity argon gas with a mass concentration of not less than 99.99% is used for coaxial protection during welding, and the flow rate of the protective gas is 10-20 L / min.

Citation Information

Patent Citations

  • Method for improving performance of aluminium alloy laser welding head

    CN108723596A

  • Aluminum alloy welding method based on SiCp / Al composite strengthening mechanism

    CN110497066A

  • Nano ceramic reinforced high-entropy alloy composite powder for additive manufacturing as well as preparation method and application thereof

    CN111168057A

  • High-entropy alloy composite powder and method for strengthening magnesium alloy through ultrahigh-speed laser cladding

    CN111996435A

  • Method for strengthening high-entropy alloy cladding layer through ceramic particles and application

    CN113493913A