Lead-free halogen-free solder wire and preparation method thereof

By adding end amino hyperbranched polyamide to the solder wire flux, the problems of reduced solder wire expansion rate and increased corrosion of substrate caused by the neutralization reaction of organic acids and organic amines are solved, and the high expansion rate of solder wire and The oxidation resistance is improved and the life of electronic products is extended.

CN119077219AActive Publication Date: 2024-12-06深圳市永佳润金属有限公司

Patent Information

Application Number
CN202411334748.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-06
Estimated Expiration
2044-09-24

AI Technical Summary

Technical Problem

The neutralization reaction between organic acids and organic amines in existing solder wire fluxes leads to a decrease in solder wire expansion rate and an increase in the corrosion of the substrate, and the solder joints are insufficient in oxidation resistance, which affects the life of electronic products.

Method used

Using end amino hyperbranched polyamide as the component of flux, the active product is formed by reacting with organic acids, slowing down the neutralization reaction, improving the expansion rate and oxidation resistance of the solder wire, and optimizing the flow of the solder wire by adjusting the flux component ratio. and film forming properties.

Benefits of technology

It significantly improves the expansion rate and splash resistance of the solder wire, reduces the corrosion of the substrate, enhances the oxidation resistance of the solder joints, and extends the life of electronic products.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of welding materials, in particular to a lead-free and halogen-free solder wire and a preparation method thereof.The lead-free and halogen-free solder wire is prepared from tin alloy and scaling powder, and the weight percentage of the added scaling powder is 4-7%; the soldering flux is prepared from the following raw materials in percentage by weight: 2-5% of an organic acid mixture, 1-5% of an organic amine mixture, 6-15% of a thixotropic agent, 2-8% of a surfactant and the balance of rosin. The organic amine mixture is prepared by mixing micromolecular organic amine and amino-terminated hyperbranched polyamide, and the weight part ratio of the micromolecular organic amine to the amino-terminated hyperbranched polyamide is 4: (0.5-2); the organic acid mixture is a mixture of adipic acid, 2-hydroxymethylbutyric acid and stearic acid; the method has the advantages that corrosion to a base material during welding is reduced, and the expansion rate of the solder wire is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of welding materials, and in particular to a lead-free and halogen-free solder wire and a preparation method thereof. Background Art

[0002] Solder wire, also known as solder wire, tin wire, tin wire, is composed of tin alloy and flux. Among them, the flux is generally a rosin resin flux composed of rosin, resin, halide activator, additives and organic carrier. Although this type of flux has low cost, stable performance and good solderability, it has strong post-welding corrosion and high ion contamination. The halogen ions in the post-welding residues are easy to cause corrosion of the surface lines of the printed circuit board, and then gradually cause the degradation of electrical insulation performance and short circuit, shortening the life of electronic products.

[0003] At present, there are lead-free solder fluxes prepared by compounding organic acids, organic amines, compounding modified rosin resins and other raw materials. Among them, organic acids are usually adipic acid, suberic acid, glutaric acid, glutaric anhydride, tetradic acid, dodecanoic acid, malic acid, etc., and organic amines include diethanolamine, triethanolamine, etc. Too much organic acid will cause high corrosion of the substrate. Therefore, organic amines not only serve as activators, but also can neutralize with organic acids and acidic residues after welding to reduce the corrosiveness of the flux. However, when the amount of organic amine added reaches a certain level, it is easy to react with the organic acid to neutralize. Some neutralization products are not decomposed into original reactants during the welding process, and the activation is insufficient, resulting in limited expansion rate of the solder wire. Summary of the invention

[0004] In order to reduce corrosion to a substrate during welding and improve the expansion rate of a solder wire, the present application provides a lead-free and halogen-free solder wire and a preparation method thereof.

[0005] In the first aspect, the present application provides a lead-free and halogen-free solder wire, which adopts the following technical solution: A lead-free and halogen-free solder wire is prepared from a tin alloy and a soldering flux, wherein the soldering flux is added in an amount of 4-7% by weight, and the soldering flux is prepared from the following raw materials in an amount of: 2-5% of an organic acid mixture, 1-5% of an organic amine mixture, 6-15% of a thixotropic agent, 2-8% of a surfactant, and the remainder is rosin; The organic amine mixture is prepared by mixing a small molecule organic amine and an amino-terminated hyperbranched polyamide, and the weight ratio of the small molecule organic amine to the amino-terminated hyperbranched polyamide is 4:(0.5-2); The organic acid mixture is a mixture of adipic acid, 2-hydroxymethylbutyric acid and stearic acid.

[0006] By adopting the above technical scheme, the amino-terminated hyperbranched polyamide is a hyperbranched polymer, which belongs to a highly branched three-dimensional macromolecule. The hyperbranched polymer has many branching points and rich terminal functional groups; its molecular chain is not easy to entangle, and the viscosity does not change with the increase of molecular weight; it has excellent fluidity and film-forming properties. The amino-terminated hyperbranched polyamide is applied to the soldering flux, and its molecular structure contains a large number of terminal amino functional groups. On the one hand, it can play an activating role as an organic amine activator. On the other hand, its reactive groups and reaction activity are stronger, and it is more preferential to neutralize with organic acids than small molecule organic amines. The neutralization product is not decomposed into the original product during the re-welding process, and its molecular structure still has active groups, and the neutralization product still has the role of an activator, thereby alleviating the problem of reduced activation and reduced solder wire expansion rate caused by the neutralization reaction of organic acids and organic amines. And its reaction with organic acids can reduce corrosion to the substrate. In addition, the addition of amino-terminated hyperbranched polyamide can slow down the flow rate of the flux, make the flux adapt to the flow rate of the tin alloy, and push the rosin to the surface of the tin alloy. After the welding is completed, the rosin can wrap the solder joint, which can increase the oxidation resistance of the solder joint. The amino-terminated hyperbranched polyamide moves to the surface of the tin alloy with the rosin and plays a role in film formation and curing, making the antioxidant film formed on the surface of the solder joint more complete, further improving the oxidation resistance of the tin alloy, and the subsequent anti-corrosion performance of the copper plate corrosion test is also better.

[0007] Preferably, the weight ratio of the small molecule organic amine to the amino-terminated hyperbranched polyamide is 4:1.

[0008] By adopting the above technical solution, the amount of amino-terminated hyperbranched polyamide added is too large, its reaction activity is high, and it reacts too much with small molecular acids, which reduces the activation performance of the flux. When the weight ratio of diethanolamine and amino-terminated hyperbranched polyamide added is 4:1, the synergistic effect between the two substances is optimal.

[0009] Preferably, the amino-terminated hyperbranched polyamide has a molecular weight of 800-1000 and contains 7-9 amino groups in a single molecule.

[0010] By adopting the above technical scheme, the synergistic effect between the terminal amino hyperbranched polyamide with a higher molecular weight and the small molecular organic amine is better, and when the molecular weight is lower, the synergistic effect is lower.

[0011] Preferably, the small molecule organic amine is diethanolamine or triethanolamine.

[0012] By adopting the above technical solution, both diethanolamine and triethanolamine can synergistically enhance the performance with the amino-terminated hyperbranched polyamide.

[0013] Preferably, the organic acid mixture is a mixture of adipic acid, 2-hydroxymethylbutyric acid and stearic acid, and the weight ratio of the organic acid mixture added is 2:1:(0.5-4).

[0014] By adopting the above technical scheme, the activation effect is better when adipic acid, 2-hydroxymethylbutyric acid and stearic acid are added within this ratio range.

[0015] Preferably, the thixotropic agent is one or more of hydrogenated castor oil, ethylene bisstearic acid amide and polyethylene wax.

[0016] By adopting the above technical solution, any type of thixotropic agent can be added within this range.

[0017] Preferably, the surfactant is one or more of rosin alcohol ether surfactant, Tween-30, AEO-9 and NP-9.

[0018] By adopting the above technical solution, the surfactant can improve the compatibility between the various substances in the flux.

[0019] Preferably, the rosin is one or both of hydrogenated rosin and hydrogenated acrylic acid modified rosin.

[0020] Preferably, the tin alloy is a tin-copper alloy or a tin-silver-copper alloy.

[0021] By adopting the above technical solution, the soldering flux of the present application is applicable to both tin-copper and tin-silver-copper alloys.

[0022] In a second aspect, the present application provides a method for preparing a lead-free and halogen-free solder wire, which adopts the following technical solution: A method for preparing a lead-free and halogen-free solder wire comprises the following steps: S1. Heat the rosin to 130-150°C and stir to melt according to the amount in Table 1, then add the organic acid mixture and stir until completely melted, then add the organic amine mixture and stir until completely dissolved, finally add the surfactant and thixotropic agent and continue stirring to obtain the flux, cool it to 120-140°C and keep it warm for later use; S2, melting the tin alloy and casting it into a hollow concentric cylindrical ingot, which is then cooled and solidified; S3, pour the soldering flux kept warm in S1 into the concentric cylindrical ingot prepared in S2 and fill it up, and after cooling, produce lead-free and halogen-free solder wire through extrusion, rolling, drawing and wire winding.

[0023] By adopting the above technical scheme, the preparation method of the present application has no special requirements for equipment, is suitable for mass production in factories, has a wide range of required technical parameters, and has a high production pass rate.

[0024] In summary, the present application includes at least one of the following beneficial technical effects: 1. The amino-terminated hyperbranched polyamide is used in the flux. Its molecular structure contains a large number of terminal amino functional groups. On the one hand, it can act as an organic amine activator to activate the organic amine. On the other hand, its reactive groups and reaction activity are stronger. It has a higher priority than small molecule organic amines in neutralization reaction with organic acids. The neutralized product does not decompose into the original product during the welding process. Its molecular structure still has active groups and the neutralized product still has the function of an activator, which can alleviate the problem of reduced activation and reduced solder wire expansion rate caused by the neutralization reaction of organic acids and organic amines. And its reaction with organic acids can reduce corrosion to the substrate. In addition, the addition of amino-terminated hyperbranched polyamide can slow down the flow rate of the flux, make the flux adapt to the flow rate of the tin alloy, and push the rosin to the surface of the tin alloy. After the welding is completed, the rosin can wrap the solder joint, which can increase the oxidation resistance of the solder joint. The amino-terminated hyperbranched polyamide moves to the surface of the tin alloy with the rosin and plays a role in film formation and curing, making the antioxidant film formed on the surface of the solder joint more complete, further improving the oxidation resistance of the tin alloy, and the subsequent anti-corrosion performance of the copper plate corrosion test is also better.

[0025] 2. The lead-free and halogen-free solder wire prepared in the present application has excellent anti-spatter performance and copper plate corrosion resistance, and its expansion rate can reach 88.1%. DETAILED DESCRIPTION

[0026] The present application is further described in detail below in conjunction with the specific contents.

[0027] raw material The raw materials used in the embodiments of the present application can all be purchased commercially; among them, the NOC (120°C ± 2h) content of the amino-terminated hyperbranched polyamide is less than 3.0%; the effective ingredient content of the polyethylene wax is 99%; the rosin alcohol ether surfactant is a premium grade product with an effective ingredient content of 99%; the grade of the hydrogenated rosin is industrial grade; the grade of the hydrogenated acrylic acid modified rosin is industrial grade. Example

[0028] Example 1 A lead-free and halogen-free solder wire is made of a tin alloy and a soldering flux, wherein the tin alloy is Sn-0.7Cu, the weight percentage of the soldering flux added is 5%, and the raw materials of the soldering flux and the amount of each raw material are shown in Table 1. The preparation method of the solder wire is as follows: S1. Heat the rosin to 140°C and stir to melt it according to the dosage in Table 1, then add the organic acid mixture and stir until it is completely melted, then add the organic amine mixture and stir until it is completely dissolved, finally add the surfactant and thixotropic agent and continue stirring for 30 minutes to obtain the flux, cool it to 140°C and keep it warm for later use; S2, melt Sn-0.7Cu and cast it into a hollow concentric cylindrical ingot, cool it to 25°C and solidify it; S3, pour the soldering flux kept warm in S1 into the concentric cylindrical ingot prepared in S2 and fill it up, cool it to 25°C, and then make lead-free and halogen-free solder wire by extrusion, rolling, drawing and winding.

[0029] The organic acid mixture is a mixture of adipic acid, 2-hydroxymethylbutyric acid and stearic acid, and the weight ratio of the organic acid mixture is 2:1:2; the organic amine mixture is a mixture of diethanolamine and amino-terminated hyperbranched polyamide, and the weight ratio of the organic acid mixture is 4:1; the thixotropic agent is polyethylene wax; the surfactant is a rosin alcohol ether surfactant, and the weight ratio of the organic acid mixture is 1:1; the rosin is a mixture of hydrogenated rosin and hydrogenated acrylic acid modified rosin, and the weight ratio of the organic acid mixture is 2:1; the relative molecular weight of the amino-terminated hyperbranched polyamide is 800-1000, and the number of amino groups contained in a single molecule is 7-9.

[0030] Table 1 Raw materials and dosage of each raw material in Example 1 soldering flux (kg) Organic acid mixture 4 Organic amine mixture 4 Thixotropic agent 10 Surfactants 5 rosin 77 Example 2 A lead-free and halogen-free solder wire is different from Example 1 in that, in its organic amine mixture, a mixture of diethanolamine and amino-terminated hyperbranched polyamide is added in a weight ratio of 4:0.5, and the remaining steps are the same as those in Example 1.

[0031] Example 3 A lead-free and halogen-free solder wire is different from Example 1 in that, in its organic amine mixture, a mixture of diethanolamine and amino-terminated hyperbranched polyamide is added in a weight ratio of 4:2, and the remaining steps are the same as those of Example 1.

[0032] Example 4 A lead-free and halogen-free solder wire is different from Example 1 in that diethanolamine in the organic amine mixture is replaced by triethanolamine in equal parts by weight, and the remaining steps are the same as those in Example 1.

[0033] Example 5 A lead-free and halogen-free solder wire is different from Example 1 in that, in its organic acid mixture, adipic acid, 2-hydroxymethylbutyric acid, and stearic acid are added in a weight ratio of 2:1:4, and the remaining steps are the same as those in Example 1.

[0034] Example 6 A lead-free and halogen-free solder wire is different from Example 1 in that, in its organic acid mixture, adipic acid, 2-hydroxymethylbutyric acid, and stearic acid are added in a weight ratio of 2:1:0.5, and the remaining steps are the same as those in Example 1.

[0035] Example 7 A lead-free and halogen-free solder wire is different from Example 1 in that its tin alloy is Sn-1.0Ag-0.5Cu, and the remaining steps are the same as those of Example 1.

[0036] Comparative Example Comparative Example 1 A lead-free and halogen-free solder wire is different from Example 1 in that no amino-terminated hyperbranched polyamide is added to the organic amine mixture, and the remaining steps are the same as those of Example 1.

[0037] Comparative Example 2 A lead-free and halogen-free solder wire is different from Example 1 in that diethanolamine is not added to the organic amine mixture, and the remaining steps are the same as those of Example 1.

[0038] Comparative Example 3 A lead-free and halogen-free solder wire is different from Example 1 in that the relative molecular weight of the amino-terminated hyperbranched polyamide added to the organic amine mixture is 350-370, the number of amino groups contained in a single molecule is 3-4, and the remaining steps are the same as those of Example 1.

[0039] Comparative Example 4 A lead-free and halogen-free solder wire is different from Example 1 in that stearic acid is not added to the organic acid mixture, and the remaining steps are the same as those of Example 1.

[0040] Performance testing Detection method / test method Lead-free and halogen-free solder wires were prepared according to the preparation methods of Examples 1-7 and Comparative Examples 1-4, and then tested according to the following testing method. The test results are shown in Table 2.

[0041] Anti-splash level: refer to the test method in SJ / T11389-2009 for testing. The lower the level, the better the anti-splash effect; Expansion rate: refer to the test method in SJ / T11390-2009 for testing; Copper plate corrosion: Corrosion refers to the chemical reaction between copper, solder and flux residues when the solder joint is exposed to 40℃ and 93%RH environment after welding. The copper plate corrosion experiment can examine the corrosion of flux residues after welding. Its judgment standard refers to IPC TM-6502.6.15C.

[0042] Table 2 Test results of Examples 1-7 and Comparative Examples 1-4 Splash protection level (level) Expansion rate (%) Copper plate corrosion Example 1 1 88.1 none Example 2 1 85.3 Slight corrosion Example 3 1 87.9 none Example 4 1 88.0 none Example 5 1 87.5 none Example 6 1 85.6 none Example 7 1 87.8 none Comparative Example 1 1 80.2 Moderate corrosion Comparative Example 2 2 74.7 none Comparative Example 3 1 76.4 Slight corrosion Comparative Example 4 1 84.9 none It can be seen from Examples 1-7 and Comparative Examples 1-4, as well as the test data in Table 2, that the lead-free and halogen-free solder wire prepared in the present application has excellent anti-spatter performance and copper plate corrosion resistance, and its expansion rate can reach 88.1%.

[0043] The amino-terminated hyperbranched polyamide is a hyperbranched polymer, which belongs to a highly branched three-dimensional macromolecule. The hyperbranched polymer has many branching points and rich terminal functional groups; its molecular chain is not easy to entangle, and the viscosity does not change with the increase of molecular weight, which is different from linear macromolecules; it has excellent fluidity and film-forming properties. Based on its structural and performance advantages, it has been used as a new functional material, such as a cross-linking agent, a nonlinear optical material, and a high-spin organic macromolecule, and shows good effects. The present application applies the amino-terminated hyperbranched polyamide to the soldering flux, and its molecular structure contains a large number of terminal amino functional groups. On the one hand, it can play a role as an organic amine active agent, and on the other hand, it is assumed that even if it undergoes a neutralization reaction with a small molecule organic acid, the neutralization product is not decomposed into the original product during the re-welding process, and its molecular structure still has an active group, and the neutralization product still has the function of an active agent, thereby alleviating the problem of reduced activation and reduced solder wire expansion rate caused by the neutralization reaction of organic acid and organic amine. And its reaction with organic acid can reduce corrosion to the substrate.

[0044] It can be seen from the test data of Example 1 and Comparative Examples 1-2 that adding a certain amount of amino-terminated hyperbranched polyamide to the flux can significantly improve the expansion rate of the solder wire. However, according to the test data of Comparative Examples 1-2, the activation performance of amino-terminated hyperbranched polyamide is not as good as that of small molecule organic amines. Therefore, it needs to be compounded with small molecule organic amines to achieve a better comprehensive effect.

[0045] When the amount of amino-terminated hyperbranched polyamide added is too large, its reactivity is high, and it reacts too much with small molecule acids, which reduces the activation performance of the flux. In combination with Example 2-3, when the weight ratio of diethanolamine and amino-terminated hyperbranched polyamide added is 4:1, the synergistic effect between the two substances is optimal.

[0046] In addition, experiments have found that the addition of amino-terminated hyperbranched polyamide can slow down the flow rate of the flux, adapt the flow rate of the flux to that of the tin alloy, and push the rosin to the surface of the tin alloy. After welding is completed, the rosin can wrap the solder joints, which can increase the oxidation resistance of the solder joints. The amino-terminated hyperbranched polyamide moves to the surface of the tin alloy with the rosin and plays a role in film formation and curing, making the antioxidant film formed on the surface of the solder joint more complete, further improving the oxidation resistance of the tin alloy, and the subsequent anti-corrosion performance of the copper plate corrosion test is also better.

[0047] It can be seen from the test data of Example 1 and Comparative Example 3 that the synergistic effect of the amino-terminated hyperbranched polyamide with a higher molecular weight and the small molecule organic amine is better. Combined with the test data of Example 4, it can be seen that the small molecule organic amine can be synergistic with diethanolamine or triethanolamine.

[0048] It can be seen from the test data of Example 1, Examples 5-6, and Comparative Example 4 that in the organic acid mixture of the present application, when the ratio of adipic acid to 2-hydroxymethylbutyric acid is constant, the addition ratio of stearic acid has a greater influence on the expansion rate of the solder wire. The optimal addition ratio is a weight ratio of adipic acid, 2-hydroxymethylbutyric acid, and stearic acid of 2:1:2.

[0049] It can be seen from the test data of Example 1 and Example 7 that the soldering flux of the present application is applicable to both tin-copper and tin-silver-copper alloys.

[0050] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.

Claims

1. A lead-free and halogen-free solder wire, Features: It is prepared from tin alloy and soldering flux, the soldering flux is added in an amount of 4-7% by weight, and the soldering flux is prepared from the following raw materials in an amount of: 2-5% organic acid mixture, 1-5% organic amine mixture, 6-15% thixotropic agent, 2-8% surfactant, and the balance is rosin; The organic amine mixture is prepared by mixing small molecule organic amine and amino-terminated hyperbranched polyamide, and the weight ratio of the small molecule organic amine to the amino-terminated hyperbranched polyamide is 4:(0.5-2); The organic acid mixture is a mixture of adipic acid, 2-hydroxymethylbutyric acid and stearic acid.

2. A lead-free and halogen-free solder wire according to claim 1, Features: The weight ratio of the small molecule organic amine to the amino-terminated hyperbranched polyamide is 4:

1.

3. A lead-free and halogen-free solder wire according to claim 1, Features: The molecular weight of the amino-terminated hyperbranched polyamide is 800-1000, and the number of amino groups contained in a single molecule is 7-9.

4. The lead-free and halogen-free solder wire according to claim 1, Features: The small molecule organic amine is diethanolamine or triethanolamine.

5. The lead-free and halogen-free solder wire according to claim 1, Features: The organic acid mixture is a mixture of adipic acid, 2-hydroxymethylbutyric acid and stearic acid, and the weight ratio of the organic acid mixture added is 2:1:(0.5-4).

6. The lead-free and halogen-free solder wire according to claim 1, Features: The thixotropic agent is one or more of hydrogenated castor oil, ethylene bisstearic acid amide and polyethylene wax.

7. The lead-free and halogen-free solder wire according to claim 1, Features: The surfactant is one or more of rosin alcohol ether surfactant, Tween-30, AEO-9 and NP-9.

8. The lead-free and halogen-free solder wire according to claim 1, Features: The rosin is one or both of hydrogenated rosin and hydrogenated acrylic acid modified rosin.

9. The lead-free and halogen-free solder wire according to claim 1, Features: The tin alloy is a tin-copper alloy or a tin-silver-copper alloy.

10. A method for preparing the lead-free and halogen-free solder wire according to any one of claims 1 to 9, Features: It includes the following steps: S1. Heat the rosin to 130-150°C and stir to melt according to the amount in Table 1, then add the organic acid mixture and stir until completely melted, then add the organic amine mixture and stir until completely dissolved, finally add the surfactant and thixotropic agent and continue stirring to obtain the flux, cool it to 120-140°C and keep it warm for later use; S2, melting the tin alloy and casting it into a hollow concentric cylindrical ingot, which is then cooled and solidified; S3, pour the soldering flux kept warm in S1 into the concentric cylindrical ingot prepared in S2 and fill it up, and after cooling, produce lead-free and halogen-free solder wire through extrusion, rolling, drawing and wire winding.

Citation Information

Patent Citations

  • Halogen-free lead-free soldering paste for radiator and preparation method thereof

    CN101695796A

  • Tin soldering paste, preparation method of tin soldering paste and welding method

    CN112894194A

  • Lead-free halogen-free anti-splashing laser solder wire and preparation method thereof

    CN114453792A

  • Lead-free and halogen-free solder paste

    US11992901B1

Cited By

  • Halogen-free soldering flux for lead-free solder wire, preparation method of halogen-free soldering flux and tin-based flux-cored wire with halogen-free soldering flux

    CN120962203A