Polishing method for casting
Through the systematic casting grinding method, targeted treatment of burrs and pit defects in investment casting is carried out, which improves the yield and surface quality of the castings, and solves the defect problems caused by low mold shell strength and complex process control. Reduced working time.
Patent Information
- Application Number
- CN202411394064.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-12-06
AI Technical Summary
Burrs and pit defects caused by low mold shell strength in investment casting, as well as inevitable defects caused by complex process control, may cause castings to be scrapped in severe cases.
Systematic casting grinding methods are adopted, including dust removal, tool status inspection, process parameter confirmation, manual identification of defect locations, targeted grinding treatment, visual inspection and fluorescence inspection, and polishing treatment to ensure that the castings meet the quality inspection standards.
It improves the yield rate of castings, reduces the working time of operators, ensures the surface quality and finish of castings, and enhances the controllability and stability of the process.
Smart Images

Figure CN119077506A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of casting grinding, and in particular to a casting grinding method. Background Art
[0002] Investment casting is an ancient casting process. The quality of the mold shell is one of the three key processes of investment casting. If the shell mold strength is low, the molten metal will break through the shell mold and enter the shell mold gap during pouring, forming burrs; if some refractory sand is mixed into the mold shell before casting, pits will be formed after casting. In addition, there are many influencing factors in investment casting, and the process control cannot be perfect. There will always be some unavoidable defects, and serious defects may cause the casting to be scrapped.
[0003] Therefore, it is necessary to provide a method for grinding a casting to solve the above problems. Summary of the invention
[0004] The purpose of the present invention is to provide a method for grinding castings, which enables operators to solve the defect problems of castings through systematic steps, improve the yield rate of castings, and reduce the working time of operators.
[0005] To achieve this object, the present invention adopts the following technical solutions:
[0006] 1. A method for grinding a casting, comprising:
[0007] S1. Turn on the dust removal device to remove dust and check the status of the grinding tool;
[0008] S2. Checking the process card of the casting to be polished to confirm the process parameters of the casting to be polished;
[0009] S3. manually marking defect positions of the casting to be polished according to the process parameters;
[0010] S4, grinding the defective position according to the type of the defect;
[0011] S5, inspect the defective position after grinding by visual inspection and / or fluorescent inspection, if the inspection is qualified, execute S6, if the inspection is unqualified, execute S4;
[0012] S6. Polishing the ground casting to make the casting meet the required roughness.
[0013] Preferably, in step S2, the process parameters include:
[0014] The reference points, machining allowances, visual inspection requirements and fluorescent inspection requirements of the casting.
[0015] Preferably, the step S4 specifically includes the following steps:
[0016] S401, determining the type of the defect, if the defect is a convex defect, executing step S402, if the defect is a concave defect, executing step S403;
[0017] S402, performing coarse grinding and fine grinding on the convex defect in sequence;
[0018] S403, polishing and repairing the concave defect.
[0019] Preferably, in step S402, a 60-mesh or 80-mesh grinding head is used to coarsely grind the raised defect.
[0020] Preferably, in step S402, the raised defect is finely ground using a short sand belt with a mesh size greater than 120 or a conical sandpaper with a mesh size greater than 120.
[0021] Preferably, in step S403, the concave defect is polished and repaired using a grinding head with a mesh greater than 100.
[0022] Preferably, in step S403, if the concave defect has oxidized inclusions, sandblasting is performed before polishing.
[0023] Preferably, the oxidation inclusions are detected by fluorescence detection.
[0024] Preferably, the concave defect is sandblasted using 60-mesh or 80-mesh blasting material to remove the oxide inclusions.
[0025] Preferably, step S6 comprises the following steps:
[0026] S601, sandblasting the casting using a 60-mesh or 80-mesh spray material;
[0027] S602, sandblasting the casting using a blasting material of a target mesh size.
[0028] Beneficial effects of the present invention:
[0029] The specific steps of the casting grinding method include: S1, open the dust removal device to remove dust, and check the state of the grinding tool; S2, check the process card of the casting to be ground, and confirm the process parameters of the casting to be ground; S3, manually mark the defect position of the casting to be ground according to the process parameters; S4, grind the defect position according to the type of defect; S5, inspect the defect position after grinding through visual inspection and / or fluorescent inspection, if the inspection is qualified, execute S6, if the inspection is unqualified, execute S4; S6, polish the casting after grinding so that the casting meets the required roughness. The dust removal device can timely clean the dust generated during the grinding process, ensure the cleanliness of the working environment, protect the health and safety of the operators, check the status of the grinding tools to prevent the grinding tools from loosening and affecting the grinding process; by checking the process card to confirm the process parameters of the casting to be polished, the grinding process has a basis to rely on, and ensure the accuracy and consistency of the grinding; the defect position is manually marked so that the grinding operation can be accurately aligned, avoid aimless grinding, and prevent the introduction of new defects; according to the defect type, targeted grinding treatment is carried out to effectively remove different types of casting defects and improve the surface quality of the casting; the defect position after grinding is detected by visual inspection and / or fluorescent inspection to ensure that the grinding effect meets the standard, timely discover and deal with unqualified situations, and ensure the controllability and stability of the grinding quality; the polished casting is polished to further improve the surface finish and roughness of the casting to meet the quality requirements. This casting grinding method uses systematic steps to enable operators to solve the defect problem of the casting accordingly, improve the yield rate of the casting, and reduce the labor time of operators. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a schematic flow chart of the casting grinding method provided by the present invention. DETAILED DESCRIPTION
[0031] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention. It should also be noted that, for ease of description, only parts related to the present invention, rather than all structures, are shown in the accompanying drawings.
[0032] In the description of the present invention, unless otherwise clearly specified and limited, the terms "connected", "connected", and "fixed" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0033] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.
[0034] In the description of this embodiment, the terms "upper", "lower", "right", etc., directions or positional relationships are based on the directions or positional relationships shown in the drawings, and are only for the convenience of description and simplification of operation, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are only used to distinguish in the description and have no special meaning.
[0035] Investment casting is an ancient casting process. The quality of the mold shell is one of the three key processes of investment casting. If the shell mold strength is low, the molten metal will break through the shell mold and enter the shell mold gap during pouring, forming burrs; if some refractory sand is mixed into the mold shell before casting, pits will be formed after casting. In addition, there are many influencing factors in investment casting, and the process control cannot be perfect. There will always be some unavoidable defects, and serious defects may cause the casting to be scrapped.
[0036] In order to solve the above problems, Figure 1 As shown, this embodiment provides a method for grinding a casting, and the specific steps include:
[0037] S1. Turn on the dust removal device to remove dust and check the status of the grinding tool;
[0038] S2. Check the process card of the casting to be polished to confirm the process parameters of the casting to be polished;
[0039] S3. Manually mark the defect positions of the casting to be polished according to the process parameters;
[0040] S4. Grind the defective position according to the type of defect;
[0041] S5, inspect the defect position after grinding by visual inspection and / or fluorescent inspection. If the inspection is qualified, execute S6; if the inspection is unqualified, execute S4;
[0042] S6. Polishing the ground casting to make the casting meet the required roughness.
[0043] The dust removal device can timely clean the dust generated during the grinding process, ensure the cleanliness of the working environment, protect the health and safety of the operators, check the status of the grinding tools to prevent the grinding tools from loosening and affecting the grinding process; by consulting the process card to confirm the process parameters of the casting to be polished, the grinding process has a basis to rely on, and ensure the accuracy and consistency of the grinding; the defect position is manually marked so that the grinding operation can be accurately aligned, avoiding aimless grinding and preventing the introduction of new defects; targeted grinding treatment is carried out according to the defect type to effectively remove different types of casting defects and improve the surface quality of the casting; the defect position after grinding is detected by visual inspection and / or fluorescent inspection to ensure that the grinding effect meets the standard, timely discover and deal with unqualified situations, and ensure the controllability and stability of the grinding quality; the polished casting is polished to further improve the surface finish and roughness of the casting to meet the quality requirements. This casting grinding method uses systematic steps to enable operators to solve the defect problem of the casting accordingly, improve the yield rate of the casting, and reduce the labor time of operators.
[0044] Specifically, the process parameters in step S2 specifically include the reference point, machining allowance, visual inspection requirements and fluorescent inspection requirements of the casting. The reference point of the casting is an important reference point on the casting for determining its position, size and shape. The reference point of the casting is not allowed to be polished to prevent the destruction of its original accuracy and positional relationship, resulting in the loss of control of the size and shape of the casting, affecting the quality and performance of the casting; the machining allowance is the thickness of the metal layer pre-set in the machining process to obtain the machining surface required by the design. The casting is polished according to the machining allowance to ensure that enough metal layer is removed to achieve the required size and shape accuracy; according to the visual inspection requirements and fluorescent inspection requirements, the operator can clearly understand which defects of the casting are allowed and which defects must be repaired, and mark the defect positions that need to be polished accordingly to ensure that the polished casting meets the requirements.
[0045] Specifically, step S4 includes the following steps:
[0046] S401, determine the type of defect, if the defect is a convex defect, execute step S402, if the defect is a concave defect, execute step S403;
[0047] S402, performing rough grinding and fine grinding on the convex defects in sequence;
[0048] S403, polishing and repairing the concave defects.
[0049] That is, when grinding defects, first determine the type of defect. For convex defects, rough grinding and fine grinding are required in sequence; for concave defects, polishing is required. By accurately and specifically grinding different types of defects, the overall quality of the casting is significantly improved, unnecessary grinding time and material consumption are reduced, thereby improving grinding efficiency and reducing production costs.
[0050] Specifically, in step S402, a 60-mesh or 80-mesh grinding head is used to rough-grind the convex defects. A 60-mesh or 80-mesh grinding head can quickly remove the convex defects, which helps to shorten the rough grinding time and improve production efficiency. Among them, the grinding head can use an aluminum oxide grinding head. It should be noted that during rough grinding, the grinding head cannot touch the casting surface around the convex defects to prevent damage to the casting surface.
[0051] Specifically, in step S402, the raised defect is finely ground using a short sand belt with a mesh greater than 120 or a conical sandpaper with a mesh greater than 120. The short sand belt or conical sandpaper with a mesh greater than 120 has finer abrasive particles, which can be further refined on the basis of rough grinding to remove tiny protrusions left by rough grinding, and can more accurately control the removal amount to ensure that the raised defect is completely repaired without excessive removal.
[0052] Specifically, in step S403, a grinding head with a mesh greater than 100 is used to polish the concave defect. A 100-mesh grinding head can better remove the rough surface around the concave defect, making the repaired surface smoother. The grinding head is an aluminum oxide grinding head or a diamond grinding head.
[0053] In this embodiment, in step S403, if there are oxidized inclusions in the concave defect, sandblasting is performed before polishing. After removing the oxidized inclusions, the subsequent polishing work will be more efficient and smooth, which helps to reduce processing time and cost.
[0054] Specifically, fluorescence was used to detect oxidation inclusions.
[0055] Specifically, 60-mesh or 80-mesh blasting material is used to blast the concave defects to remove oxide inclusions. The 60-mesh blasting material has relatively large particles and is suitable for occasions where a large number of oxide inclusions need to be removed quickly; the 80-mesh blasting material can maintain a good surface texture while removing oxide inclusions and avoid excessive damage to the surrounding intact metal surface. The mesh number of the blasting material can be selected according to the specific situation and treatment requirements of the concave defect. Specifically, the blasting material is corundum sand.
[0056] Specifically, step S6 includes the following steps:
[0057] S601, use 60 mesh or 80 mesh spray material to sandblast the casting;
[0058] S602, sandblasting the casting using a blasting material of a target mesh size.
[0059] First, the casting is sandblasted with a 60-mesh or 80-mesh blasting material to cover the scratches left by grinding, quickly improve the basic state of the casting surface, and make the roughness of the casting surface basically uniform; then the casting is sandblasted with a target mesh blasting material to further refine the surface so that the surface roughness of the casting meets the target requirements. Specifically, the blasting material is corundum sand.
[0060] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, various obvious changes, readjustments and substitutions can be made without departing from the protection scope of the present invention. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for grinding a casting, characterized in that: include: S1. Turn on the dust removal device to remove dust and check the status of the grinding tool; S2. Checking the process card of the casting to be polished to confirm the process parameters of the casting to be polished; S3. manually marking defect positions of the casting to be polished according to the process parameters; S4, grinding the defective position according to the type of the defect; S5, inspect the defective position after grinding by visual inspection and / or fluorescent inspection, if the inspection is qualified, execute S6, if the inspection is unqualified, execute S4; S6. Polishing the ground casting to make the casting meet the required roughness.
2. The method for grinding a casting according to claim 1, characterized in that: In step S2, the process parameters include: The reference points, machining allowances, visual inspection requirements and fluorescent inspection requirements of the casting.
3. The method for grinding a casting according to claim 1, characterized in that: The step S4 specifically includes the following steps: S401, determining the type of the defect, if the defect is a convex defect, executing step S402, if the defect is a concave defect, executing step S403; S402, sequentially performing rough grinding and fine grinding on the convex defect; S403, polishing and repairing the concave defect.
4. The method for grinding a casting according to claim 3, characterized in that: In the step S402, the convex defect is roughly ground using a 60-mesh or 80-mesh grinding head.
5. The method for grinding a casting according to claim 4, characterized in that: In the step S402, the raised defect is finely ground using a short sand belt with a mesh size greater than 120 or a conical sandpaper with a mesh size greater than 120.
6. The method for grinding a casting according to claim 3, characterized in that: In the step S403, the concave defect is polished and repaired using a grinding head with a mesh greater than 100.
7. The method for grinding a casting according to claim 6, characterized in that: In the step S403, if the concave defect has oxidized inclusions, sandblasting is performed before polishing.
8. The method for grinding a casting according to claim 7, characterized in that: The oxidative inclusions were detected by fluorescence examination.
9. The method for grinding a casting according to claim 7, characterized in that: The concave defect is sandblasted using 60-mesh or 80-mesh blasting material to remove the oxide inclusions.
10. The method for grinding a casting according to claim 1, characterized in that: The step S6 comprises the following steps: S601, sandblasting the casting using a 60-mesh or 80-mesh spray material; S602, sandblasting the casting using a blasting material of a target mesh size.
Citation Information
Cited By
Polishing process for door plate of control cabinet
CN119526137A