Fiber pretreatment method and application of treated fiber
By using dimethylacetamide and lithium chloride solution to treat fibers in fiberboard production, combined with hot pressing molding technology, the problem of acid and alkali pretreatment destroying the fiber structure is solved, and the mechanical properties and water resistance of glue-free plywood fiberboard are significantly improved. .
Patent Information
- Application Number
- CN202411378107.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-30
AI Technical Summary
In the production of existing fiberboards, acid-base pretreatment methods will destroy the crystalline structure of the fiber, affect the mechanical properties and water resistance, and there are problems of equipment corrosion and chemical reagent residues, resulting in poor performance of glue-free fiberboards.
Use dimethylacetamide to dissolve fibers, add lithium chloride solution for heating treatment and physically extrude and remove reagents, rinse and dry water to obtain pre-treated fibers, and prepare glue-free plywood fiberboard by hot pressing to adjust the fiber surface structure to Improve self-gluing performance.
The mechanical properties and water resistance of glue-free plywood fiberboard are significantly improved. The fibrillation of cellulose greatly increases the self-gluing interface. The self-gluing cooperation of degradation products of cellulose and lignin is improved, and the overall performance of the board is improved.
Smart Images

Figure CN119077881A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fiberboard preparation, and more particularly to a fiber pretreatment method and application of the treated fiber. Background Art
[0002] my country is the largest producer and consumer of fiberboard, with an annual output of 50 million cubic meters. 90% of fiberboard production uses urea-formaldehyde resin adhesives, which poses a risk of formaldehyde pollution. A small number of fiberboards use isocyanate adhesives, but they have problems such as high cost and easy cracking. Based on the dual requirements of the environment and economy, the development of glue-free plywood has become an urgent need for green production and quality and efficiency improvement of the fiberboard industry under the "dual carbon" strategy.
[0003] Glue-free plywood refers to a man-made fiberboard made by hot pressing wood fiber or other plant fiber without adding any adhesive. Since the fiber relies on its own bonding force during the hot pressing process to form a board, and the fiber itself has a low adhesive content, pretreatment is required in the early stage. The commonly used acid-base pretreatment method will destroy the fiber crystal structure and affect the fiber performance, resulting in the mechanical properties and water resistance of the glue-free fiberboard being incomparable to those of traditional fiberboard. In addition, the acid-base pretreatment will also cause certain corrosion to the equipment, and the pretreatment chemical reagents will remain in the fiber, causing the glue-free fiberboard to degrade too quickly in the acid-base environment, affecting the life of the fiberboard.
[0004] Therefore, green and sustainable fiber pretreatment technology and preparation methods of high-performance glue-free plywood still need to be developed. Summary of the invention
[0005] In view of this, the present invention provides a recyclable fiber pretreatment method and application of the treated fibers, which changes the surface structure through pretreatment and is applied to fiberboard preparation to obtain a glue-free plywood with excellent mechanical properties and water resistance.
[0006] To achieve the above object, the present invention adopts the following technical solution:
[0007] First, the present invention provides a fiber pretreatment method, comprising the following steps:
[0008] (1) placing the fiber in dimethylacetamide at room temperature to decompose it, thereby obtaining decomposed fiber;
[0009] (2) dissolving lithium chloride in dimethylacetamide to obtain a solution;
[0010] (3) placing the debonded fibers in step (1) in the solution of step (2), heating the solution for a period of time and then cooling the solution to room temperature for further treatment;
[0011] (4) Physically squeezing the fibers treated in step (3) to remove the reagent, washing the filtered fibers with water, and then drying to obtain pretreated fibers.
[0012] Preferably, the fiber in step (1) comprises one or more of eucalyptus fiber, poplar fiber, fir fiber, masson pine fiber, miscellaneous wood fiber, and bamboo fiber, more preferably poplar fiber and moso bamboo fiber.
[0013] Preferably, in step (1), the material-liquid ratio of fiber to dimethylacetamide is 1 g:10 mL to 1 g:100 mL, and the decomposition time is 2 h to 12 h, more preferably the material-liquid ratio is 1 g:50 mL, and the decomposition time is 6 h to 8 h.
[0014] The effects of the above preferred technical solution are: if the material-liquid ratio is too low, it is difficult to completely wet the fibers and the debonding effect is poor; if it is too high, it will cause solvent waste.
[0015] Preferably, in step (2), the mass fraction of lithium chloride in dimethylacetamide is 5% to 8%, more preferably 6% to 7%.
[0016] Preferably, in step (3), the material-liquid ratio of the deflated fibers to the solution is 1g:10mL to 1g:100mL, more preferably 1g:50mL, and the treatment process is firstly treated at 80°C to 90°C for 1h to 2h, preferably at 85°C for 1.5h; and then cooled to room temperature for 12 to 18h.
[0017] The effects of the above preferred technical solution are: if the material-liquid ratio is too low, it is difficult to completely infiltrate the fiber during the treatment process; if it is too high, the permeability of the solution on the fiber surface will be too high, which will seriously damage the crystallinity of the surface cellulose and reduce the self-bonding performance. If the treatment time is too short, the cellulose on the fiber surface will be dissolved and regenerated into fewer fibrils, making it difficult to form strong hydrogen bonds; if the time is too long, more surface cellulose will be dissolved, the overall crystallinity of the fiber will be affected, and the self-bonding performance will be reduced. Therefore, a reasonable material-liquid ratio and treatment time are defined to ensure the optimal debonding effect.
[0018] Preferably, in step (4), the drying is carried out by airing or drying at 40°C to 60°C to a moisture content of 8% to 12%, and the drying temperature is more preferably 50°C and the moisture content is 10%.
[0019] The effect of the above preferred technical solution is: the treated fiber is used for the production of glue-free plywood. During the production process, too high drying temperature causes serious fiber agglomeration, which is not conducive to fiber laying and will lead to uneven density of self-plywood; too low drying temperature takes too long to dry the fiber, thereby increasing manufacturing energy consumption; airing is an energy-saving drying method, but it is not the best solution due to the long time. In addition, when hot pressing is performed to prepare glue-free fiberboard at a high moisture content of 8% to 12%, the presence of water molecules can destroy the hydrogen bonding of cellulose in the fiber, which is conducive to releasing the hydroxyl sites on the surface of cellulose and generating more hydrogen bonding with the cellulose on the surface of the activated fiber. At the same time, water molecules play an interfacial transition role during the hot pressing volatilization process, promoting the formation of a solid-liquid stable interface to a solid-solid interface. However, if the moisture content is too high, it is difficult to remove the moisture in a short hot pressing time, resulting in bubbling of the self-plywood, while if the moisture content is too low, it is difficult to play the role of water molecules.
[0020] The present invention also provides a pretreated fiber obtained by the method described in the above technical solution.
[0021] The present invention also provides a pretreated fiber obtained by the method described in the above scheme or the use of the pretreated fiber in preparing glue-free plywood.
[0022] Furthermore, the application includes the following steps: breaking up and laying out the pretreated fibers, and hot pressing and forming.
[0023] Preferably, the pavement thickness is 2mm to 12mm and the density is 0.8 to 1.2g / cm 3 , hot pressing temperature is 150℃~190℃, hot pressing pressure is 4~8MPa, and hot pressing time is 2~4mm / min.
[0024] More preferably, the hot pressing temperature is 180° C. and the time is 3 mm / min.
[0025] The effect of the above preferred technical solution is: the improvement of the self-bonding performance of the fiber depends on two factors. First, the lignin and hemicellulose in the fiber are degraded at a certain temperature and humidity to form small molecules, and the degradation products are self-bonded. Second, cellulose is melted and regenerated to form filaments on the fiber surface, and the surface fibrillation greatly increases the hydroxyl group and activity of the fiber surface, and the hydroxyl group forms hydrogen bonds to improve the self-bonding performance.
[0026] Therefore, if the hot pressing temperature is too low, lignin and hemicellulose are difficult to degrade, and the self-adhesive properties of the degradation products decrease. However, if the hot pressing temperature is too high, it is easy to cause carbonization of the fiber surface and blackening of the self-adhesive fiberboard.
[0027] Similarly, hot pressing pressure is also a very important factor. If the hot pressing pressure is too low, it will be difficult for the hydroxyl groups on the fibrillated surface to form strong hydrogen bonds. The boards formed with weak hydrogen bonds will easily absorb water and expand under high humidity conditions, affecting the performance of the self-adhesive boards.
[0028] It can be seen from the above technical solutions that, compared with the prior art, the present invention discloses a fiber pretreatment method and application of the treated fiber in preparing fiberboard, which has the following beneficial effects:
[0029] After treatment with LiCl / DMAc solution, the hemicellulose and lignin on the fiber surface are decomposed, cellulose is dissolved, and cellulose is regenerated after water washing, forming cellulose fibrils on the fiber surface, which greatly increases the area of the self-bonding interface and the activity of the surface hydroxyl groups. In the process of glue-free bonding, not only the degradation products of hemicellulose and lignin are self-bonded, but also the cellulose fibrils are self-bonded under the action of hydrogen bonds. The three major components in the fiber play their own self-bonding role, which significantly improves the performance of glue-free plywood. Among them, the treatment time, temperature, and concentration of LiCl / DMAc solution are important influencing factors. If the concentration is too low, the temperature is too low, or the time is too short, the cellulose is difficult to dissolve. If the concentration is too high, the temperature is too high, or the time is too long, the cellulose will dissolve too much, which will destroy the crystallization of cellulose and reduce the mechanical strength of the fiber. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0031] Figure 1 Schematic diagram of the difference between fiber before and after pretreatment;
[0032] Figure 2 The following are scanning electron micrographs of wood fiber before and after pretreatment. DETAILED DESCRIPTION
[0033] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] In the following examples and comparative examples, the static bending strength test process of the prepared plate is as follows:
[0035] Cut the plate into a size of 5mm×60mm×t (t is thickness), adjust the support span of the mechanical testing machine to at least 20 times the thickness of the specimen, place the specimen on the support, with the long axis of the specimen perpendicular to the supporting roller and the center point of the specimen under the loading roller, load the entire specimen at a constant speed, adjust the loading speed, reach the maximum load within 1 minute, record the maximum load, and take the average value of 5 parallel tests.
[0036] Static bending strength formula:
[0037] σ: static bending strength of specimen, MPa;
[0038] F max : Maximum load when the specimen is damaged, N;
[0039] l: distance between two supports, mm;
[0040] b: specimen width, mm;
[0041] t: specimen thickness, mm.
[0042] The elastic modulus test method of the prepared plate is the same as that of the static bending strength.
[0043] Elastic modulus formula:
[0044] E b : elastic modulus of the specimen, MPa;
[0045] l: distance between two supports, mm;
[0046] b: specimen width, mm;
[0047] t: specimen thickness, mm;
[0048] F2-F1: the increase of load in the straight line segment of the load-deflection curve, N;
[0049] a2-a1: The increase in deformation in the middle of the specimen, that is, the deformation of the specimen in the force range F2 to F1, mm.
[0050] The test method for the water absorption expansion rate of the prepared board is:
[0051] Cut the board into 20mm×20mm size, immerse it in a water tank with a pH value of 7±1 and a temperature of (20±1)℃, with the upper part of the specimen below the water surface by (25±5)mm. Soak for 24h. After immersion, take out the specimen, wipe off the water attached to the surface, and measure its thickness at the original measuring point. The water absorption expansion rate is the ratio of the increase in thickness after water absorption to the thickness before water absorption.
[0052] Water absorption expansion formula:
[0053] T: water absorption thickness expansion rate, %;
[0054] t1: thickness of the specimen before immersion, mm;
[0055] t2: Thickness of specimen after immersion in water, mm.
[0056] Example 1
[0057] (1) 16 g of poplar fiber was placed in 800 mL of dimethylacetamide (DMAc) and dissolved at room temperature for 6 h;
[0058] (2) dissolving lithium chloride (LiCl) in DMAc to prepare 800 mL of a 6% LiCl / DMAc solution;
[0059] (3) placing the poplar wood fibers decomposed in step (1) in the solution of step (2), treating at 85° C. for 1 h, then cooling to room temperature and continuing the treatment for 12 h;
[0060] (4) physically squeezing the poplar fiber treated in step (3) to remove LiCl / DMAc, recovering the LiCl / DMAc reagent for reuse, washing and filtering the poplar fiber with water, and drying the poplar fiber in an oven at 50° C. to a moisture content of 8%;
[0061] (5) Spread the dried poplar fibers and lay them out. The mold size is 100 mm × 100 mm × 2 mm, and the density is 0.8 g / cm 3 , hot pressing temperature is 150℃, hot pressing temperature is 150℃, hot pressing pressure is 4MPa, hot pressing time is 1min, and glue-free poplar fiberboard is obtained.
[0062] The obtained poplar fiberboard was tested:
[0063] Static bending strength: 36MPa;
[0064] Elastic modulus: 3.2GPa;
[0065] 24h moisture expansion rate: 8%.
[0066] Example 2
[0067] (1) 50 g of bamboo fiber was placed in 2000 mL of dimethylacetamide (DMAc) and dissolved at room temperature for 7 h;
[0068] (2) dissolving lithium chloride (LiCl) in DMAc to prepare 2000 mL of a 7% LiCl / DMAc solution;
[0069] (3) placing the bamboo fiber decomposed in step (1) in the solution of step (2), treating at 85° C. for 1.5 h, cooling to room temperature and continuing the treatment for 15 h;
[0070] (4) physically squeezing the bamboo fiber in step (3) to remove LiCl / DMAc, recovering the LiCl / DMAc for reuse, washing and filtering the bamboo fiber with water, and drying the bamboo fiber in the sun until the moisture content is 10%;
[0071] (5) Spread the dried bamboo fibers and lay them out. The mold size is 100 mm × 100 mm × 5 mm, and the density is 1.0 g / cm 3 , hot pressing temperature is 180℃, hot pressing pressure is 5MPa, hot pressing time is 2.5min, and glue-free bonded bamboo fiberboard is obtained.
[0072] The obtained bamboo fiberboard was tested:
[0073] Static bending strength: 96MPa;
[0074] Elastic modulus: 12GPa;
[0075] 24h moisture expansion rate: 3%.
[0076] Example 3
[0077] (1) 120 g of Chinese fir fiber was placed in 1200 mL of dimethylacetamide (DMAc) and dissolved at room temperature for 8 h;
[0078] (2) dissolving lithium chloride (LiCl) in DMAc to prepare 1200 mL of 8% LiCl / DMAc solution;
[0079] (3) placing the fir fiber decomposed in step (1) in the solution of step (2), treating at 90° C. for 2 h, then cooling to room temperature and continuing the treatment for 18 h;
[0080] (4) physically squeezing the poplar fiber treated in step (3) to remove LiCl / DMAc, recovering the LiCl / DMAc reagent for reuse, washing and filtering the fir fiber with water, and drying the fir fiber in an oven at 50° C. to a moisture content of 12%;
[0081] (5) Spread the dried fir fiber, 100mm×100mm×10mm, density 1.2g / cm 3 , hot pressing temperature is 190℃, hot pressing pressure is 6MPa, hot pressing time is 2.5min, and glue-free glued fir fiberboard is obtained.
[0082] The obtained fir fiberboard was tested:
[0083] Static bending strength: 110MPa;
[0084] Elastic modulus: 15GPa;
[0085] 24h moisture expansion rate: 2.5%.
[0086] Example 4
[0087] (1) 50 g of poplar fiber was placed in 5000 mL of dimethylacetamide (DMAc) and dissolved at room temperature for 7 h;
[0088] (2) dissolving lithium chloride (LiCl) in DMAc to prepare 5000 mL of a 7% LiCl / DMAc solution;
[0089] (3) placing the poplar wood fibers defragmented in step (1) in the solution of step (2), treating at 85° C. for 1.5 h, then cooling to room temperature and continuing the treatment for 15 h;
[0090] (4) physically squeezing the poplar fiber treated in step (3) to remove LiCl / DMAc, recovering the LiCl / DMAc reagent for reuse, washing and filtering the poplar fiber with water, and drying the poplar fiber in an oven at 50° C. to a moisture content of 12%;
[0091] (5) Spread the dried poplar fibers and spread them out. Spread the dried poplar fibers and spread them out. The mold size is 100 mm × 100 mm × 5 mm, and the density is 1.0 g / cm 3 The hot pressing temperature is 180°C, the hot pressing pressure is 8MPa, and the hot pressing time is about 1.6min to obtain a glue-free poplar fiberboard.
[0092] The obtained poplar fiberboard was tested:
[0093] Static bending strength: 104MPa;
[0094] Elastic modulus: 11GPa;
[0095] 24h moisture expansion rate: 2.8%.
[0096] Comparative Example 1
[0097] Poplar wood fibers that have not been treated with LiCl / DMAc solution were used to prepare fiberboard using the method of Example 4. The test results are as follows:
[0098] Static bending strength: 55MPa;
[0099] Elastic modulus: 2GPa;
[0100] 24h moisture expansion rate: 25%.
[0101] Comparative Example 2
[0102] The difference from Example 4 is that the hot pressing temperature is 100°C. The test results are:
[0103] Static bending strength: 73MPa;
[0104] Elastic modulus: 5GPa;
[0105] 24h moisture expansion rate: 11%.
[0106] Comparative Example 3
[0107] The difference from Example 4 is that the hot pressing temperature is 200°C. The test results are:
[0108] Black surface
[0109] Static bending strength: 54MPa;
[0110] Elastic modulus: 12GPa
[0111] 24h moisture expansion rate: 2%.
[0112] Comparative Example 4
[0113] The difference from Example 4 is that the drying is performed to a moisture content of 7%. The test results are as follows:
[0114] Static bending strength: 79MPa;
[0115] Elastic modulus: 6GPa;
[0116] 24h moisture expansion rate: 9%.
[0117] Comparative Example 5
[0118] The difference from Example 4 is that the drying is performed to a moisture content of 13%. The test results are as follows:
[0119] Bubbling;
[0120] Static bending strength: 44MPa;
[0121] Elastic modulus: 4GPa;
[0122] 24h moisture expansion rate: 19%.
[0123] Experimental Example 1
[0124] The fibers treated in Example 4 and the untreated fibers in Comparative Example 1 were tested. The results are shown in the attached figure. Figure 2 As shown, Figure 2 In the figure, the upper two figures are the fiber morphology pictures of the untreated comparative example 1, and the lower two figures are the fiber morphology pictures after being treated by embodiment 4. It can be seen from the figures that the surface of the treated fibers is rough and fibrillated, the cellulose fibrils are exposed, and the surface hydroxyl groups increase, while the surface of the untreated fibers is smooth.
[0125] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments, and the same and similar parts between the embodiments can be referred to each other. The above description of the disclosed embodiments enables professionals and technicians in this field to implement or use the present invention. Various modifications to these embodiments will be obvious to professionals and technicians in this field, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to these embodiments shown in this article, but will comply with the widest range consistent with the principles and novel features disclosed herein.
Claims
1. A fiber pretreatment method, characterized in that: The following steps are involved: (1) placing the fiber in dimethylacetamide at room temperature to decompose it, thereby obtaining decomposed fiber; (2) dissolving lithium chloride in dimethylacetamide to obtain a solution; (3) placing the debonded fibers in step (1) in the solution of step (2), heating the solution for a period of time and then cooling the solution to room temperature for further treatment; (4) Physically squeezing the fibers treated in step (3) to remove the reagent, washing the filtered fibers with water, and then drying to obtain pretreated fibers.
2. A fiber pretreatment method according to claim 1, characterized in that: The fiber in step (1) includes one or more of eucalyptus fiber, poplar fiber, fir fiber, masson pine fiber, miscellaneous wood fiber and bamboo fiber.
3. A fiber pretreatment method according to claim 1, characterized in that: In step (1), the material-liquid ratio of the fiber to dimethylacetamide is 1 g:10 mL to 1 g:100 mL, and the disintegration time is 2 h to 12 h.
4. A fiber pretreatment method according to claim 1, characterized in that: In step (2), the mass fraction of lithium chloride in dimethylacetamide is 5% to 8%.
5. A fiber pretreatment method according to claim 1, characterized in that: In step (3), the material-liquid ratio of the decomposed fiber and the solution is 1g:10mL~1g:100mL, and the treatment process is firstly treated at 80℃~90℃ for 1h~2h, and then cooled to room temperature for 12~18h.
6. A fiber pretreatment method according to claim 1, characterized in that: In step (4), the drying is carried out by airing in the sun or drying at 40°C to 60°C to a moisture content of 8% to 12%.
7. A pretreated fiber obtained by the method according to any one of claims 1 to 6.
8. Use of the pretreated fiber obtained by the method according to any one of claims 1 to 6 or the pretreated fiber according to claim 7 in the preparation of glue-free plywood.
9. The use according to claim 8, characterized in that: The following steps are involved: The pretreated fibers are spread out and laid out, and then hot-pressed into shape.
10. The use according to claim 8, characterized in that: Pavement thickness 2mm~12mm, density 0.8~1.2g / cm 3 , hot pressing temperature is 150℃~190℃, hot pressing pressure is 4~8MPa, and hot pressing time is 2~4mm / min.
Citation Information
Patent Citations
Method of using non-adhesive method to prepare cellulose base fiber
CN101550614A
Preparation method and application of cellulose solution
CN108250460A
Preparation method for softening and bending wood
CN112157751A
Method for forming high-strength and formaldehyde-release-free plywood through adhesive-free and self-adhesion
CN113001696A
Preparation method of high-strength and high-toughness recyclable fiberboard with bionic structure and cyclic treatment method of high-strength and high-toughness recyclable fiberboard
CN117144706A
Cited By
Fiber pretreatment method for preparing binderless fiberboard
CN120503290A