Tg140 lead-free copper-clad plate material with low solvent usage amount and preparation process of Tg140 lead-free copper-clad plate material

A Tg140 lead-free copper clad laminate material is produced using a modified epoxy resin system with cyanate resin and fillers, addressing solvent-related environmental issues and ensuring high mechanical properties, thus meeting green production and performance standards.

CN119078338AActive Publication Date: 2024-12-06JIANGXI GAOSHUO HANGYU NEW MATERIALS CO LTD

Patent Information

Application Number
CN202411004516.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-12-06
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The use of large amounts of organic solvents in the production of copper clad laminates leads to environmental risks and increased recycling costs, while conventional resin glue systems fail to meet the requirements of high performance and green production.

Method used

A Tg140 lead-free copper clad laminate material is prepared using a curing system composed of brominated epoxy resin, polyamic acid modified epoxy resin, bismaleimide modified epoxy resin, and liquid crystal modified epoxy resin, combined with cyanate resin and phenolic resin, along with a wetting agent and inorganic/organic fillers, to reduce solvent usage while maintaining mechanical properties.

Benefits of technology

The process significantly reduces solvent usage by 25%-35%, enhancing mechanical properties such as peel strength and bending strength, thus meeting green production standards and performance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a Tg140 lead-free copper-clad plate material with low solvent consumption and a preparation process thereof, and belongs to the technical field of copper-clad plates. According to the process, brominated epoxy resin, polyamic acid modified epoxy resin, bismaleimide modified epoxy resin, liquid crystal modified epoxy resin, cyanate ester resin and phenolic resin are used as raw materials, a wetting agent, organic filler and the like are matched to prepare a resin glue solution, a bonding sheet is obtained after glass fiber cloth is impregnated, and finally the bonding sheet and copper foil are combined and pressed to obtain the copper-clad plate. The use amount of the organic solvent required for preparing the resin glue solution can be remarkably reduced, the excellent mechanical property of the copper-clad plate can be ensured, and a new way is provided for preparing the green and environment-friendly high-performance copper-clad plate with high peel strength and high bending strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of copper clad laminates, and in particular relates to a Tg140 lead-free copper clad laminate material with low solvent usage and a preparation process thereof. Background Art

[0002] With the rapid development of electronic appliances, people have put forward more and more requirements for printed circuit boards, involving requirements such as compactness, multi-function, lead-free, halogen-free and green production, which undoubtedly puts higher requirements on the production process of copper clad laminates.

[0003] Copper clad laminate, also known as copper foil laminate, is the core material for making printed circuit boards, responsible for the conductive, insulating and supporting functions of printed circuit boards. Copper clad laminate is made of wood pulp paper or glass fiber cloth as reinforcing materials, impregnated with resin glue, and made into a bonding sheet. After combining several bonding sheets, copper foil is applied on one or both sides, and then cured by hot pressing to form a plate-like material. Based on this, resin glue is the key to affecting many performance indicators of copper clad laminates, and its raw material selection and preparation process have become the focus of copper clad laminate production.

[0004] Resin glue is generally made of different resins or resin mixtures, mixed with fillers, etc., and then added with organic solvents to make "glue"; resin glue directly affects the various properties between the bonding sheets. In order to adjust the dispersion properties and viscosity of different resin compositions and fillers, etc., a variety of organic solvents are often used as the regulating solvents of the resin mixture in the field, and the amount used is huge. The use of a large amount of solvent will increase the amount of solvent volatilization in the later stage, thereby causing greater environmental risks and increasing recycling costs. Therefore, how to effectively reduce the amount of solvent used in the process while ensuring the mechanical properties of the copper clad laminate has become a problem that needs to be solved urgently in green production. Summary of the invention

[0005] In view of the content of the background technology, the purpose of the present invention is to provide a Tg140 lead-free copper clad laminate material with low solvent usage and a preparation process thereof. The process of the present invention uses brominated epoxy resin, polyamic acid modified epoxy resin, bismaleimide modified epoxy resin, liquid crystal modified epoxy resin, cyanate resin, phenolic resin to construct a curing system, and cooperates with a wetting agent and an organic filler, which not only greatly reduces the amount of resin glue solvent, but also can ensure the mechanical properties of the copper clad laminate, and has good market competitiveness.

[0006] In order to achieve the above object, the present invention specifically adopts the following technical solutions: The present invention provides a preparation process of a Tg140 lead-free copper clad laminate material with a low solvent usage, comprising the following steps: Step 1: adding an epoxy resin mixture and a wetting agent to an inorganic filler, mixing, high-speed shearing at 30-50° C., adding an organic filler, a cyanate resin, and a phenolic resin to the obtained mixture, mixing evenly, and adjusting the viscosity with a solvent to obtain a resin glue; the epoxy resin mixture is composed of brominated epoxy resin, polyamic acid modified epoxy resin, bismaleimide modified epoxy resin, and liquid crystal modified epoxy resin; Step 2: impregnating the glass fiber cloth with the resin glue obtained in step 1, and then baking at 180-210° C. to obtain a bonding sheet; Step 3: Combine several adhesive sheets obtained in step 2, coat one or both sides with copper foil, and then press them together to form a Tg140 lead-free copper clad laminate material.

[0007] Preferably, the raw materials in step 1 are calculated by weight as follows: 90-110 parts of epoxy resin mixture, 15-25 parts of cyanate resin, 45-70 parts of phenolic resin, 15-20 parts of inorganic filler, 4-6 parts of organic filler, 2-5 parts of wetting agent, and sufficient solvent.

[0008] Preferably, the epoxy resin mixture is composed of brominated epoxy resin, polyamic acid modified epoxy resin, bismaleimide modified epoxy resin and liquid crystal modified epoxy resin in a mass ratio of (5-8):(1-2):(1-2):1.

[0009] Preferably, the preparation method of the polyamic acid modified epoxy resin is: polyamic acid and E51 epoxy resin are mixed in a mass ratio of 1:3, a catalyst and a solvent are added, the temperature is raised to 80-90° C., and the mixture is stirred at a constant temperature for 3-5 h. After removing impurities, the polyamic acid modified epoxy resin is obtained.

[0010] Preferably, the preparation method of the bismaleimide-modified epoxy resin is: bismaleimide and E51 epoxy resin are mixed in a mass ratio of 1:4, a catalyst and a solvent are added, the temperature is raised to 100-110° C., and the mixture is stirred at a constant temperature for 5-7 h. After impurities are removed, the bismaleimide-modified epoxy resin is obtained.

[0011] Preferably, the preparation method of the liquid crystal modified epoxy resin is: blending a thermotropic liquid crystal polymer with 2-3 times the mass of PSU, heating the resulting mixture to melt, then adding it to 15-25 times the mass of E44 epoxy resin that has been heated to the same temperature in advance, mixing at a constant temperature, cooling and adding a curing agent and a catalyst to obtain a liquid crystal modified epoxy resin.

[0012] Preferably, the inorganic filler is at least one of aluminum hydroxide, white carbon black, silicon carbide, titanium oxide and kaolin; and the organic filler is organic tin acetate.

[0013] Preferably, the wetting agent is polyethylene glycol octylphenyl ether.

[0014] Tg is a key indicator for measuring heat resistance, which indirectly affects the mechanical, electrical, chemical and other properties of copper clad laminates. The process of the present invention uses a variety of modified resins as raw materials to prepare a Tg140 lead-free copper clad laminate with low solvent usage. The present invention uses brominated epoxy resin as the main resin. The brominated epoxy resin has excellent heat resistance, electrical insulation and adhesion. The main curing system constructed with phenolic resin can maintain the basic viscosity of the glue and the basic strength and heat resistance of the bonding sheet. In addition, the process of the present invention uses polyamic acid and bismaleimide to modify E51 type epoxy resin respectively. Polyamic acid can form an ester-like structure with epoxy groups when modifying epoxy resin. Its own activity can also be amidated to form a long chain with bismaleimide, so that the curing system shows high bonding shear strength and heat resistance. The combination of the two can not only promote compatibility and significantly improve the bonding strength of the glue at high temperature, but also strengthen the peeling performance of the system. Thermotropic liquid crystal polymer contains liquid crystal unit, and the epoxy resin modified by the same can further compensate for the brittleness of the matrix and enhance the comprehensive mechanical properties without affecting the mechanical properties. Cyanate resin has good high temperature mechanical properties, bending strength, dimensional stability and stable dielectric properties. The present invention also adds a special wetting agent and inorganic / organic composite filler, polyethylene glycol octylphenyl ether and organic tin acetate can promote the dispersibility of inorganic filler and mixed resin, and can further enhance the compatibility between resin systems, which not only effectively reduces the use of organic solvent in resin glue, but also gives excellent mechanical properties to the glue after curing.

[0015] Compared with the prior art, the present invention has the following beneficial effects: The present invention overcomes the defect that the resin glue system prepared by conventional epoxy resin and inorganic filler cannot meet the requirements of high performance and green production. A variety of modified epoxy resins are used in conjunction with cyanate resin and phenolic resin to construct a main curing system, and a wetting agent and an organic filler are used. At the same time, the amount of raw materials and the preparation process are optimized. This can not only significantly reduce the amount of organic solvent required for preparing the resin glue, but also ensure the excellent mechanical properties of the copper clad laminate, thereby providing a new way to prepare green and environmentally friendly high-performance copper clad laminates with high peel strength and high bending strength. DETAILED DESCRIPTION

[0016] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0017] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0018] Example 1 A preparation process of Tg140 lead-free copper clad laminate material: 1. Add maleic anhydride to the DMF solution of 4,4'-diaminodiphenyl ether in several portions, and mix thoroughly in a water bath at 60°C to obtain polyamic acid; mix 100 parts by weight of polyamic acid with 300 parts by weight of E51 epoxy resin, add 1.2 parts by weight of triphenylphosphine and an appropriate amount of DMF, heat to 85°C, stir at constant temperature for 4 hours, and then remove impurities in a vacuum to obtain polyamic acid-modified epoxy resin. Mix 100 parts by weight of bismaleimide with 400 parts by weight of E51 epoxy resin, add 0.5 parts by weight of dibutyltin dilaurate and an appropriate amount of DMA, heat to 105°C, stir at constant temperature for 5.5 hours, and then remove impurities in a vacuum to obtain bismaleimide-modified epoxy resin. 1.5 parts by weight of Xydar II (Amoco, USA) and 3.5 parts by weight of PSU (GF-1006) were blended and heated to melt as a modifier and kept at a constant temperature. 100 parts by weight of E44 epoxy resin was heated to the same temperature and mixed with the modifier at a constant temperature for 30 min. Then the temperature was lowered to 145°C, 3 parts by weight of 2-methylimidazole and 0.8 parts by weight of DMP-30 were added, and the reaction was continued for 2 h to obtain a liquid crystal modified epoxy resin.

[0019] 2. Weigh by weight 60 parts of brominated epoxy resin NPEB-400, 15 parts of the above-mentioned polyamic acid modified epoxy resin, 15 parts of the above-mentioned bismaleimide modified epoxy resin, 10 parts of the above-mentioned liquid crystal modified epoxy resin, 20 parts of cyanate resin, 55 parts of phenolic resin 2123, 9 parts of aluminum hydroxide, 7 parts of white carbon black, 5 parts of organic tin acetate, and 3.5 parts of polyethylene glycol octylphenyl ether.

[0020] 3. Add brominated epoxy resin NPEB-400, liquid crystal modified epoxy resin, polyamic acid modified epoxy resin, bismaleimide modified epoxy resin and polyethylene glycol octylphenyl ether to aluminum hydroxide and white carbon black in turn, mix them, and high-speed shear at 40°C. Then, add organic tin acetate, cyanate resin and phenolic resin 2123 to the obtained mixture and mix them evenly. Add a sufficient amount of a solvent mixed with propylene glycol methyl ether and butanone of equal mass to adjust the viscosity to 20 s (the final solvent dosage is 55 parts) to obtain a resin glue. Use the obtained resin glue to coat glass fiber cloth (7628, 0.173 mm thick, 204.4 g / m2 per unit area) 2) for impregnation and baked at 195°C until the resin content is 48% to obtain an adhesive sheet; 8 adhesive sheets are overlapped with 2 copper foils (1oz, the same below) and pressed into a copper clad laminate with a thickness of 1.6 mm.

[0021] Example 2 A preparation process of Tg140 lead-free copper clad laminate material: 1. Add maleic anhydride to the DMF solution of 4,4'-diaminodiphenyl ether in several portions, and mix thoroughly in a water bath at 60°C to obtain polyamic acid; mix 100 parts by weight of polyamic acid with 300 parts by weight of E51 epoxy resin, add 1.4 parts by weight of triphenylphosphine and an appropriate amount of DMF, heat to 85°C, stir at constant temperature for 3 hours, and then remove impurities in a vacuum to obtain polyamic acid-modified epoxy resin. Mix 100 parts by weight of bismaleimide with 400 parts by weight of E51 epoxy resin, add 0.6 parts by weight of dibutyltin dilaurate and an appropriate amount of DMA, heat to 105°C, stir at constant temperature for 5 hours, and then remove impurities in a vacuum to obtain bismaleimide-modified epoxy resin. 1.3 parts by weight of Xydar II (Amoco, USA) and 3.9 parts by weight of PSU (GF-1006) were blended and heated to melt as a modifier and kept at a constant temperature. 100 parts by weight of E44 epoxy resin was heated to the same temperature and mixed with the modifier at a constant temperature for 30 min. Then the temperature was lowered to 145°C, 3 parts by weight of 2-methylimidazole and 0.8 parts by weight of DMP-30 were added, and the reaction was continued for 2 h to obtain a liquid crystal modified epoxy resin.

[0022] 2. Weigh by weight 60 parts of brominated epoxy resin NPEB-400, 20 parts of the above-mentioned polyamic acid modified epoxy resin, 20 parts of the above-mentioned bismaleimide modified epoxy resin, 10 parts of the above-mentioned liquid crystal modified epoxy resin, 15 parts of cyanate resin, 65 parts of phenolic resin 2123, 9 parts of aluminum hydroxide, 7 parts of white carbon black, 5 parts of organic tin acetate, and 3.5 parts of polyethylene glycol octylphenyl ether.

[0023] 3. Add brominated epoxy resin NPEB-400, liquid crystal modified epoxy resin, polyamic acid modified epoxy resin, bismaleimide modified epoxy resin and polyethylene glycol octylphenyl ether to aluminum hydroxide and white carbon black in turn, mix them, high-speed shear at 40°C, add organic tin acetate, cyanate resin and phenolic resin 2123 to the obtained mixture, mix them evenly, add a sufficient amount of a solvent mixed with propylene glycol methyl ether and butanone of equal mass to adjust the viscosity to 20 s (the final solvent dosage is 63 parts), and obtain a resin glue; use the obtained resin glue to coat glass fiber cloth (7628, 0.173 mm thick, 204.4 g / m per unit area) 2 ) for impregnation, and baked at 195°C until the resin content is 48% to obtain an adhesive sheet; 8 adhesive sheets are stacked with 2 copper foils and pressed into a copper clad laminate with a thickness of 1.6 mm.

[0024] Example 3 A preparation process of Tg140 lead-free copper clad laminate material: 1. Add maleic anhydride to the DMF solution of 4,4'-diaminodiphenyl ether in several portions, and mix thoroughly in a water bath at 60°C to obtain polyamic acid; mix 100 parts by weight of polyamic acid with 300 parts by weight of E51 epoxy resin, add 1 part by weight of triphenylphosphine and an appropriate amount of DMF, heat to 85°C, stir at constant temperature for 5 hours, and then remove impurities in a vacuum to obtain polyamic acid-modified epoxy resin. Mix 100 parts by weight of bismaleimide with 400 parts by weight of E51 epoxy resin, add 0.5 parts by weight of dibutyltin dilaurate and an appropriate amount of DMA, heat to 100°C, stir at constant temperature for 6.5 hours, and then remove impurities in a vacuum to obtain bismaleimide-modified epoxy resin. 1.8 parts by weight of Xydar II (Amoco, USA) and 3.6 parts by weight of PSU (GF-1006) were blended, heated to melt as a modifier and kept at a constant temperature. 120 parts by weight of E44 epoxy resin was heated to the same temperature and mixed with the modifier at a constant temperature for 30 minutes. Then the temperature was lowered to 145°C, 3 parts by weight of 2-methylimidazole and 0.8 parts by weight of DMP-30 were added, and the reaction was continued for 2 hours to obtain a liquid crystal modified epoxy resin.

[0025] 2. Weigh by weight 72 parts of brominated epoxy resin NPEB-400, 12 parts of the above-mentioned polyamic acid modified epoxy resin, 12 parts of the above-mentioned bismaleimide modified epoxy resin, 12 parts of the above-mentioned liquid crystal modified epoxy resin, 25 parts of cyanate resin, 45 parts of phenolic resin 2123, 9 parts of aluminum hydroxide, 7 parts of white carbon black, 4 parts of organic tin acetate, and 4 parts of polyethylene glycol octylphenyl ether.

[0026] 3. Add brominated epoxy resin NPEB-400, liquid crystal modified epoxy resin, polyamic acid modified epoxy resin, bismaleimide modified epoxy resin and polyethylene glycol octylphenyl ether to aluminum hydroxide and white carbon black in turn, mix them, high-speed shear at 40°C, add organic tin acetate, cyanate resin and phenolic resin 2123 to the mixture, mix them evenly, add enough propylene glycol methyl ether and butanone mixed with equal mass of solvent to adjust the viscosity to 20 s (final solvent dosage 58 parts), and obtain resin glue; use the obtained resin glue to coat glass fiber cloth (7628, thickness 0.173 mm, unit area mass 204.4 g / m 2 ) for impregnation, and baked at 195°C until the resin content is 48% to obtain an adhesive sheet; 8 adhesive sheets are stacked with 2 copper foils and pressed into a copper clad laminate with a thickness of 1.6 mm.

[0027] Comparative Example 1 Refer to the step parameters of Example 1, except that no polyamic acid-modified epoxy resin is added, that is: The epoxy resin mixture used is composed of 70.6 parts of brominated epoxy resin NPEB-400, 17.6 parts of bismaleimide modified epoxy resin in Example 1, and 11.8 parts of liquid crystal modified epoxy resin in Example 1.

[0028] Among them, the amount of solvent used to adjust the viscosity of the resin glue to 20 s is 84 parts.

[0029] Comparative Example 2 Refer to the step parameters of Example 1, except that no liquid crystal modified epoxy resin is added, that is: The epoxy resin mixture used is composed of 66.6 parts of brominated epoxy resin NPEB-400, 16.7 parts of polyamic acid modified epoxy resin in Example 1, and 16.7 parts of bismaleimide modified epoxy resin in Example 1.

[0030] Among them, the amount of solvent used to adjust the viscosity of the resin glue to 20 s is 77 parts.

[0031] Comparative Example 3 Refer to the step parameters of Example 1, except that no cyanate resin is added, that is: The raw materials used are as follows: 60 parts of brominated epoxy resin NPEB-400, 15 parts of polyamic acid modified epoxy resin of Example 1, 15 parts of bismaleimide modified epoxy resin of Example 1, 10 parts of liquid crystal modified epoxy resin of Example 1, 20 parts of cyanate resin, 55 parts of phenolic resin 2123, 9 parts of aluminum hydroxide, 7 parts of white carbon black, 5 parts of organic tin acetate, and 3.5 parts of polyethylene glycol octylphenyl ether.

[0032] Among them, the amount of solvent used to adjust the viscosity of the resin glue to 20 s is 85 parts.

[0033] Comparative Example 4 Refer to the step parameters of Example 1, except that organic tin acetate is not used as filler, that is: Only inorganic fillers are used - 12 parts of aluminum hydroxide and 9 parts of white carbon black.

[0034] Among them, the amount of solvent used to adjust the viscosity of the resin glue to 20 s is 84 parts.

[0035] Comparative Example 5 The step parameters are as in Example 1, except that the wetting agent polyethylene glycol octylphenyl ether is not used.

[0036] Among them, the amount of solvent used to adjust the viscosity of the resin glue to 20 s is 79 parts.

[0037] Test example The samples prepared in the above-mentioned Examples 1-3 and Comparative Examples 1-5 were subjected to performance testing (IPC-TM-650), and the results are shown in Table 1.

[0038] Table 1

[0039] In summary, the glue system of the present invention can effectively reduce the amount of solvent by 25%-35%, greatly reducing environmental risks and subsequent recycling costs of the process. At the same time, the prepared copper clad laminate has excellent peel strength, bending strength, etc., and excellent mechanical properties, meeting green production and people's various requirements for printed circuit boards.

[0040] The embodiments described above only express several preferred embodiments of the present invention, and the descriptions thereof are relatively specific and detailed, but are not intended to limit the present invention. It should be noted that for those skilled in the art, the present invention may also have various changes and modifications, and any modifications, equivalent substitutions, improvements, etc. made within the concept and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A preparation process of Tg140 lead-free copper clad laminate material with low solvent usage, characterized in that: The steps include: Step 1: adding an epoxy resin mixture and a wetting agent to an inorganic filler, mixing, high-speed shearing at 30-50° C., adding an organic filler, a cyanate resin, and a phenolic resin to the obtained mixture, mixing evenly, and adjusting the viscosity with a solvent to obtain a resin glue; the epoxy resin mixture is composed of brominated epoxy resin, polyamic acid modified epoxy resin, bismaleimide modified epoxy resin, and liquid crystal modified epoxy resin; Step 2: impregnating the glass fiber cloth with the resin glue obtained in step 1, and then baking at 180-210° C. to obtain a bonding sheet; Step 3: Assemble several adhesive sheets obtained in step 2, coat one or both sides with copper foil, and then press them together to form a Tg140 lead-free copper clad laminate material.

2. The preparation process of Tg140 lead-free copper clad laminate material with low solvent usage according to claim 1, characterized in that: The raw materials in step 1 are calculated by weight as follows: 90-110 parts of epoxy resin mixture, 15-25 parts of cyanate resin, 45-70 parts of phenolic resin, 15-20 parts of inorganic filler, 4-6 parts of organic filler, 2-5 parts of wetting agent, and sufficient amount of solvent.

3. The preparation process of Tg140 lead-free copper clad laminate material with low solvent usage according to claim 1, characterized in that: The epoxy resin mixture is composed of brominated epoxy resin, polyamic acid modified epoxy resin, bismaleimide modified epoxy resin and liquid crystal modified epoxy resin in a mass ratio of (5-8):(1-2):(1-2):

1.

4. The preparation process of Tg140 lead-free copper clad laminate material with low solvent usage according to claim 1, characterized in that: The preparation method of the polyamic acid modified epoxy resin is as follows: polyamic acid and E51 epoxy resin are mixed in a mass ratio of 1:3, a catalyst and a solvent are added, the temperature is raised to 80-90° C., and the mixture is stirred at a constant temperature for 3-5 h. After impurities are removed, the polyamic acid modified epoxy resin is obtained.

5. The preparation process of Tg140 lead-free copper clad laminate material with low solvent usage according to claim 1, characterized in that: The preparation method of the bismaleimide-modified epoxy resin is as follows: bismaleimide and E51 epoxy resin are mixed in a mass ratio of 1:4, a catalyst and a solvent are added, the temperature is raised to 100-110° C., and the mixture is stirred at a constant temperature for 5-7 h. After impurities are removed, the bismaleimide-modified epoxy resin is obtained.

6. The preparation process of Tg140 lead-free copper clad laminate material with low solvent usage according to claim 1, characterized in that: The preparation method of the liquid crystal modified epoxy resin is as follows: a thermotropic liquid crystal polymer is mixed with PSU of 2-3 times its mass, the obtained mixture is heated to melt, and then added to E44 epoxy resin of 15-25 times its mass which is heated to the same temperature in advance, mixed at a constant temperature, and a curing agent and a catalyst are added at a lower temperature to obtain the liquid crystal modified epoxy resin.

7. The process for preparing Tg140 lead-free copper clad laminate material with low solvent usage according to claim 1, characterized in that: The inorganic filler is at least one of aluminum hydroxide, white carbon black, silicon carbide, titanium oxide and kaolin; the organic filler is organic tin acetate.

8. The process for preparing Tg140 lead-free copper clad laminate material with low solvent usage according to claim 1, characterized in that: The wetting agent is polyethylene glycol octylphenyl ether.

9. The Tg140 lead-free copper clad laminate material obtained by the preparation process according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Resin composition, bonding sheet and copper-clad plate made using same, manufacturing method thereof

    CN101885900A

  • Resin composition and preparation method thereof

    CN102719096A

  • Environmental-friendly, flexible, heat-conducting epoxy resin adhesive and high-heat-conduction flexible base material prepared by using same

    CN103450836A

  • Modified alumina composite material, copper-coated substrate and preparation method of copper-coated substrate

    CN104371274A

Cited By

  • Bismaleimide-based dielectric composition for embedded capacitor and preparation method of bismaleimide-based dielectric composition

    CN121964384A