Method for improving forming quality of polyester drawn yarn

By adjusting the surface roughness and position of the friction roller, the brake mark problem in the winding molding of polyester draft wire is solved, and the uniform stress and stress distribution of the silk cake is achieved, and the forming quality is improved.

CN119079675AActive Publication Date: 2024-12-06TONGKUN GRP ZHEJIANG HENGTONG CHEM FIBER
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411422083.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-12-06
Estimated Expiration
2044-10-12

AI Technical Summary

Technical Problem

During the winding and forming process of polyester draft wire, brake marks and other problems are prone to occur, which leads to slightly collapse during the unwinding process of the silk cake, bringing out multiple circles of wire, affecting the quality and efficiency of weaving. The existing technology optimizes the winding tension, etc. The process parameters were not completely resolved.

Method used

By controlling the surface roughness of the friction roller and the relative position between the friction roller and the spindle, the surface roughness of the friction roller is gradually reduced from 0.8±0.2μm in the middle to 0.1±0.02μm in the left and right edges, and in the Y-axis direction, Offset is 0.07~0.1mm, and the X-axis direction is offset ≤0.09mm, so as to distribute the contact pressure evenly to reduce stress unevenness.

Benefits of technology

It effectively reduces the occurrence of brake marks, ensures the uniform stress and stress distribution of the silk cake during winding, and improves the molding quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079675A_ABST
    Figure CN119079675A_ABST
Patent Text Reader

Abstract

The invention relates to a method for improving the forming quality of polyester drawn yarns, which is characterized in that in the winding forming process of the polyester drawn yarns for warp knitting, the surface roughness of a friction roller and the relative position between the friction roller and a spindle shaft are controlled, so that the forming quality of the polyester drawn yarns is improved; in the axial direction, the friction roller corresponding to each spinning cake is sequentially divided into a left area, a middle area and a right area, the middle area accounts for 55-60%, and the left area and the right area respectively account for 20-22.5%; the roughness Ra of the surface of the friction roller in the middle area is 0.8 + / -0.2 mu m, and the roughness Ra of the surface of the friction roller is gradually reduced to 0.1 + / -0.02 mu m from the middle area to the left area and the right area. The stress of each point of the spinning cake is uniform, the stress distribution is more uniform, and the phenomenon that brake patterns are formed due to collapse of partial layers caused by overlarge local stress is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyester drawn yarns and relates to a method for improving the molding quality of polyester drawn yarns. Background Art

[0002] Warping is a post-process of polyester drawn yarn, which is mainly used in conjunction with warp knitting machines. When weaving on warp knitting machines, it is necessary to go through the warping stage first. In this stage, hundreds of FDY fibers are drawn out from the bobbins on the creel through the warping machine, unwound in parallel and evenly according to the specified length, and wound on the warp beam or weaving beam for subsequent sizing or weaving.

[0003] During the warping process, the FDY fiber needs to be unwound onto the warp beam or weaving beam, but residual stress will be generated when the polyester drawn yarn is wound and formed, which will lead to problems such as brake marks. When the yarn cake is unwound to the brake mark collapse layer during the unwinding process, it is easy to bring out the slightly collapsed part, so that 2 or even more turns of yarn are brought out together, that is, delamination problems will occur, which will cause unwinding knotting problems, thereby affecting the quality and efficiency of subsequent weaving.

[0004] Reference 1 (Technical Analysis of Winding Forming [J]. Synthetic Fibers, 2005(1):29-30) and Reference 2 (Analysis of Winding Forming Problems of Stretch Texturing Machine [J]. 2006(5):30-32) both describe the use of shaping rollers for high-speed spinning FDY. The solution to the forming problem mainly relies on optimizing the winding tension. However, since the spinning winder has been expanded from the original 8 heads to 16 heads, it is no longer possible to completely solve abnormal forming problems such as brake marks simply by optimizing process parameters such as winding tension.

[0005] Therefore, it is of great significance to study a method for improving the molding quality of polyester drawn yarn to solve the problems existing in the prior art. Summary of the invention

[0006] The purpose of the invention is to solve the problems existing in the prior art and provide a method for improving the molding quality of polyester drawn yarn.

[0007] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] A method for improving the forming quality of polyester drawn yarns, in which the surface roughness of a friction roller and the relative position between the friction roller and a spindle are controlled in the winding forming process of the polyester drawn yarns for warp knitting, thereby improving the forming quality of the polyester drawn yarns;

[0009] Along the axial direction, the friction roller corresponding to each silk cake is divided into three areas: left, middle and right. The middle area accounts for 55-60%, and the left and right areas account for 20-22.5% respectively. The roughness Ra of the friction roller surface in the middle area is 0.8±0.2μm. From the middle area to the left and right areas, the roughness Ra of the friction roller surface gradually decreases to 0.1±0.02μm.

[0010] Let the end of the spindle used to load the paper tube be end face a, and the other end be end face b. Establish a spatial rectangular coordinate system with the straight line passing through end face a and parallel to the horizontal plane as the X-axis, the straight line passing through end face a and perpendicular to the horizontal plane as the Y-axis, and the straight line parallel to the center axis of the spindle as the Z-axis. Let the center of the spindle end face a be the origin, and the coordinates be (0, 0, 0). The end of the friction roller close to end face a is offset upward along the Y-axis direction by 0.07~0.1mm. An offset value greater than 0.1mm or less than 0.07mm will be on the wire. During the initial winding stage and after the cake grows to a certain extent, one end of the friction roller will be out of contact with the silk cake. When the offset value is greater than 0.1mm, the end face b will be out of contact with the friction roller in the initial winding stage and the contact pressure will be less than the set value, resulting in excessive local stress in the silk cake. When the offset value is less than 0.07mm, the contact pressure of the friction roller at one end of the silk cake on the end face a will decrease or even be out of contact with the friction roller in the middle and late stages of winding, resulting in an increase in the intrinsic stress of the silk cake, and the offset along the X-axis direction will be less than or equal to 0.09mm.

[0011] Y axis offset = Y a -Y b ;Offset in the X-axis direction = X a , where X a is the X-axis coordinate value of the center of the friction roller near the end surface a, Y a Y is the Y-axis coordinate value of the center of the friction roller near the end surface a. b It is the Y-axis coordinate value of the center of the circle on one end of the friction roller close to the end surface b.

[0012] As the preferred technical solution:

[0013] As described above, a method for improving the forming quality of polyester drawn yarn is provided, wherein the left and right areas on the friction roller corresponding to each silk cake are equally divided into four small areas, the roughness Ra of the four small areas from right to left in the left area are 0.6±0.2μm, 0.4±0.1μm, 0.2±0.05μm, and 0.1±0.02μm, respectively, and the roughness Ra of the four small areas from left to right in the right area are 0.6±0.2μm, 0.4±0.1μm, 0.2±0.05μm, and 0.1±0.02μm, respectively.

[0014] In the method for improving the forming quality of polyester drawn yarn as described above, the spindle shaft length is 1150~1800mm.

[0015] In the method for improving the forming quality of polyester drawn yarn as described above, the number of yarn cakes arranged on the spindle shaft is 8 to 16.

[0016] In the method for improving the forming quality of polyester drawn yarn as described above, the yarn cake winding diameter ranges from 360 to 380 mm.

[0017] In the method for improving the forming quality of polyester drawn yarn as described above, the length of the friction roller is equal to that of the spindle shaft, and the diameter of the friction roller is 84.5-85.5 mm.

[0018] According to the method for improving the forming quality of polyester drawn yarn as described above, the downgrade rate of brake marks on the wound yarn cake is ≤0.1%.

[0019] Principle of the invention:

[0020] During the winding process of polyester drawn yarn, the factors that affect the winding process mainly include friction rollers, shift forks, etc.

[0021] The friction roller rotates at a constant speed, and the spindle is driven by a motor to wind and form. The surface linear speed of the friction roller is consistent with the surface linear speed of the silk cake wound on the spindle, and the friction roller contacts the surface of the silk cake with a certain pressure, so that the silk cake has a certain hardness and strength to meet the requirements of post-processing. The friction roller and the spindle shaft should be parallel in theory, but since 8 to 16 silk cakes need to be arranged on the spindle shaft, the end without physical support (i.e. the end loaded with the paper roll) will sink slightly during the process of winding the silk cake due to the increase in the weight of the silk cake. The larger the winding diameter, the greater the impact of the parallelism deviation between the friction roller and the spindle shaft caused by this sinking on the silk cake forming. During the winding and forming process, the polyester drawn yarn will be simultaneously subjected to the contact pressure applied by the friction roller and the centripetal pressure generated by the outer layer of the silk cake to the inner layer. When the spindle shaft sinks and vibrates, the residual stress caused by the uneven contact pressure and the centripetal pressure generated by the outer layer of the silk cake to the inner layer will be inconsistent, resulting in brake marks.

[0022] In order to reduce the vibration caused by the sinking of the a-end of the spindle during the increase of the weight of the silk cake and ensure that each silk cake is well formed, it is necessary to overcome the problem of increased flexibility as the weight of the spindle increases. Therefore, the present invention optimizes the parallelism (the angle between the friction roller and the spindle) so that one end of the friction roller (the same end of the spindle shaft without physical support) is offset upward by 0.07~0.1mm along the Y-axis direction, with a slightly upward angle. In this way, there will be a certain parallelism deviation in the initial stage of winding. Because this deviation has almost no effect on the initial winding formation, as the package grows, the parallelism deviation gradually returns to parallelism due to the influence of the weight of the silk cake; and the X-axis direction offset value is designed to be ≤0.09mm. The X-axis direction offset will cause the contact surface between the silk bundle and the friction roller to change, resulting in a change in the contact pressure, and then the residual stress caused by the uneven pressure is inconsistent. If the offset is ≤0.09mm, the contact pressure between the silk bundles can be guaranteed to be the same.

[0023] During the winding process, the two stacked forks rotate clockwise and counterclockwise respectively to drive the filament bundle to do reciprocating motion, so that the filaments are tightly wound around the paper tube surface in a spiral form layer by layer. However, if the friction coefficient of the friction roller surface is the same, there will be more circles in the middle of the silk cake than at the edge during the winding process. This is because the silk first passes through the wire guide hook on the winding head, then reaches the position of the two stacked forks, and then passes through the friction roller and winds around the paper tube. The wire guide hook is located in the vertical direction of the center of the paper tube. If there is no left and right movement of the fork, the silk will be wound around the center of the paper tube due to a certain tension. It is precisely because of the fork that the silk is dispersed and wound on the paper tube; however, because the silk has a certain tension, if the friction coefficient of the friction roller surface is the same, when the silk is pushed to the edge by the fork, the silk has the largest force in the horizontal direction toward the center due to tension, and this force is the smallest when the silk is in the center, resulting in the silk staying the least time when it is pushed to both sides, and the closer to the middle, the more time it stays, that is, during the winding process, the silk cake has more circles in the middle than at the edge. As the winding continues, the diameter of the silk cake increases and the middle part is higher than the two sides, resulting in uneven contact force between the friction roller and the silk cake, with the middle part being larger and the two sides being smaller, or even the contact pressure on the two sides being 0. Due to the small pressure of the friction roller, the internal stress of the two edges will increase, and the edge collapse will be serious. A slight collapse will be seen as brake marks on the side. The present invention changes the wire grabbing force by changing the smoothness of the friction roller surface, so that the centripetal force in the lateral direction of the wire is as uniform as possible during the pulling process.

[0024] The present invention redesigns the friction roller. In order to improve the wire grabbing force of the friction roller, 55-60% of the area in the middle of the friction roller corresponding to each silk cake is designed as a friction surface with a roughness Ra of 0.8±0.2μm, and the remaining 20-22.5% areas on the left and right sides gradually change from friction surfaces to smooth surfaces with roughness Ra of 0.6±0.2μm, 0.4±0.1μm, 0.2±0.05μm, and 0.1±0.02μm, respectively. The friction roller designed in this way can allow the silk to be evenly distributed at any point of the silk cake during the winding process, so that the contact between the friction roller and the silk cake is very uniform and close during the growth of the winding diameter, the force at each point of the silk cake is uniform, the stress distribution is more uniform, and the brake marks will not be formed due to the collapse of some layers due to excessive local (edge) stress.

[0025] Beneficial effects:

[0026] (1) A method for improving the forming quality of polyester drawn yarn of the present invention controls the surface roughness of the friction roller and the relative position between the friction roller and the spindle shaft, so that each point of the yarn cake is subjected to uniform force, and the stress distribution is more uniform, and brake marks are not formed due to the collapse of some layers caused by excessive local (edge) stress;

[0027] (2) A method for improving the forming quality of polyester drawn yarn of the present invention optimizes the parallelism (the angle and position between the friction roller and the spindle shaft), allows one end of the friction roller to be offset upward by 0.07-0.1 mm along the Y-axis direction, and designs the offset value in the X-axis direction to be ≤0.09 mm, thereby avoiding the influence of parallelism deviation on the forming of the yarn cake. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a side view of the friction roller and the spindle shaft;

[0029] Figure 2 It is the front view of the friction roller and the spindle shaft;

[0030] Among them, 1-friction roller, 2-spindle shaft;

[0031] Figure 1 In the figure, X1 and X2 represent the X-axis direction, and Y1 and Y2 represent the Y-axis direction;

[0032] Figure 2 Middle, Y 1A , Y 2A , Y 1B , Y 2B Indicates the Y-axis direction, Z 1A , Z 2A , Z 1B , Z 2B Represents the Z-axis direction, where A corresponds to end surface a and B corresponds to end surface b. DETAILED DESCRIPTION

[0033] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0034] Braking pattern downgrade ratio: The internal stress of the silk cake is uneven due to vibration, which causes some end faces to collapse slightly and form spiral textures, which are called braking patterns. The spiral texture exceeds the end face of the silk cake by 1mm and needs to be downgraded. Braking pattern downgrade ratio = number of downgraded pieces × 100% / total number of pieces.

[0035] Example 1

[0036] A method for improving the forming quality of polyester drawn yarn, the specific process is as follows:

[0037] In the winding process of polyester drawn yarn for warp knitting, the surface roughness of the friction roller and the relative position between the friction roller and the spindle are controlled to improve the forming quality of the polyester drawn yarn;

[0038] The spindle shaft length is 1150mm, the number of silk cakes arranged on the spindle shaft is 8; the silk cake winding diameter is 360mm;

[0039] The friction roller corresponds to the spindle shaft one by one, and the friction roller is located directly above the spindle shaft, and the length of the friction roller is equal to that of the spindle shaft; the diameter of the friction roller is 84.5 mm; along the axial direction, the friction roller corresponding to each silk cake is divided into three areas: left, middle, and right, with the middle area accounting for 60%, and the left and right areas accounting for 20% respectively; the surface roughness Ra of the friction roller in the middle area is 0.8 μm;

[0040] The left and right areas of the friction roller corresponding to each silk cake are equally divided into four small areas. The roughness Ra of the four small areas from right to left in the left area are 0.6μm, 0.4μm, 0.2μm, and 0.1μm respectively, and the roughness Ra of the four small areas from left to right in the right area are 0.6μm, 0.4μm, 0.2μm, and 0.1μm respectively.

[0041] like Figure 1~2 As shown, one end of the spindle shaft 2 for loading the paper tube is denoted as end face a, and the other end is denoted as end face b. A spatial rectangular coordinate system is established with a straight line passing through end face a and parallel to the horizontal plane as the X-axis, a straight line passing through end face a and perpendicular to the horizontal plane as the Y-axis, and a straight line parallel to the center axis of the spindle shaft as the Z-axis. The end of the friction roller 1 close to the end face a is offset upward by 0.07 mm along the Y-axis direction and by 0.05 mm along the X-axis direction.

[0042] The downgrade rate of brake marks on wound silk cakes is 0.05%.

[0043] Comparative Example 1

[0044] A method for improving the forming quality of polyester drawn yarn is basically the same as that of Example 1, except that: the surface roughness of the friction roller is consistent, which is 0.8 μm;

[0045] The downgrade rate of brake marks on wound silk cakes is 1.35%.

[0046] Compared with Example 1, the percentage of brake marks on the wound silk cakes increased significantly in Comparative Example 1. This is because the roughness of the friction roller surface in Comparative Example 1 is consistent. As the diameter of the silk cake increases, the surface of the silk cake becomes higher in the middle than on the two sides, resulting in uneven contact force between the friction roller and the silk cake. Since the pressure of the friction roller on both ends is too small, the internal stress on the two edges will increase, and brake marks of collapsed condition will appear on the two edges, thus significantly increasing the percentage of brake marks on the wound silk cakes.

[0047] Comparative Example 2

[0048] A method for improving the forming quality of polyester drawn yarn is basically the same as that of Example 1, except that: the end of the friction roller close to the end surface a is offset upward by 0.12 mm along the Y-axis direction and by 0.10 mm along the X-axis direction;

[0049] The downgrade rate of brake marks on wound silk cakes was 1.01%.

[0050] Compared with Example 1, the percentage of brake marks on the wound silk cake in Comparative Example 2 increases significantly. This is because in Comparative Example 2, the end of the friction roller close to the end face a is offset upward by 0.12 mm along the Y-axis direction and by 0.10 mm along the X-axis direction, which causes the contact pressure between the silk cake and the friction roller to decrease or even to break away from the contact with the friction roller during winding, resulting in excessive local stress in the silk cake and the appearance of brake marks.

[0051] Example 2

[0052] A method for improving the forming quality of polyester drawn yarn, the specific process is as follows:

[0053] In the winding process of polyester drawn yarn for warp knitting, the surface roughness of the friction roller and the relative position between the friction roller and the spindle are controlled to improve the forming quality of the polyester drawn yarn;

[0054] The spindle length is 1380mm, the number of silk cakes arranged on the spindle is 10; the silk cake winding diameter is 370mm;

[0055] The friction roller corresponds to the spindle shaft one by one, and the friction roller is located directly above the spindle shaft, and the length of the friction roller is equal to that of the spindle shaft; the diameter of the friction roller is 84.5 mm; along the axial direction, the friction roller corresponding to each silk cake is divided into three areas: left, middle, and right, with the middle area accounting for 58%, and the left and right areas accounting for 21% respectively; the surface roughness Ra of the friction roller in the middle area is 0.9 μm;

[0056] The left and right areas of the friction roller corresponding to each silk cake are equally divided into four small areas. The roughness Ra of the four small areas from right to left in the left area are 0.7μm, 0.5μm, 0.25μm, and 0.12μm respectively, and the roughness Ra of the four small areas from left to right in the right area are 0.7μm, 0.5μm, 0.25μm, and 0.12μm respectively.

[0057] Let one end of the spindle shaft for loading the paper tube be end face a, and the other end be end face b. Establish a spatial rectangular coordinate system with the straight line passing through end face a and parallel to the horizontal plane as the X-axis, the straight line passing through end face a and perpendicular to the horizontal plane as the Y-axis, and the straight line parallel to the center axis of the spindle shaft as the Z-axis. The end of the friction roller close to end face a is offset upward by 0.08 mm along the Y-axis direction and by 0.06 mm along the X-axis direction.

[0058] The downgrade rate of brake marks on wound silk cakes is 0.06%.

[0059] Example 3

[0060] A method for improving the forming quality of polyester drawn yarn, the specific process is as follows:

[0061] In the winding process of polyester drawn yarn for warp knitting, the surface roughness of the friction roller and the relative position between the friction roller and the spindle are controlled to improve the forming quality of the polyester drawn yarn;

[0062] The spindle shaft length is 1520mm, the number of silk cakes arranged on the spindle shaft is 12; the silk cake winding diameter is 372mm;

[0063] The friction roller corresponds to the spindle shaft one by one, and the friction roller is located directly above the spindle shaft, and the length of the friction roller and the spindle shaft are equal; the diameter of the friction roller is 85mm; along the axial direction, the friction roller corresponding to each silk cake is divided into three areas: left, middle and right, with the middle area accounting for 57%, and the left and right areas accounting for 21.5% respectively; the surface roughness Ra of the friction roller in the middle area is 1μm;

[0064] The left and right areas of the friction roller corresponding to each silk cake are equally divided into four small areas. The roughness Ra of the four small areas from right to left in the left area are 0.8μm, 0.5μm, 0.25μm, and 0.10μm respectively, and the roughness Ra of the four small areas from left to right in the right area are 0.8μm, 0.5μm, 0.25μm, and 0.10μm respectively.

[0065] Let one end of the spindle shaft for loading the paper tube be end face a, and the other end be end face b. Establish a spatial rectangular coordinate system with the straight line passing through end face a and parallel to the horizontal plane as the X-axis, the straight line passing through end face a and perpendicular to the horizontal plane as the Y-axis, and the straight line parallel to the center axis of the spindle shaft as the Z-axis. The end of the friction roller close to end face a is offset upward by 0.08 mm along the Y-axis direction and by 0.07 mm along the X-axis direction.

[0066] The downgrade rate of brake marks on wound silk cakes is 0.06%.

[0067] Example 4

[0068] A method for improving the forming quality of polyester drawn yarn, the specific process is as follows:

[0069] In the winding process of polyester drawn yarn for warp knitting, the surface roughness of the friction roller and the relative position between the friction roller and the spindle are controlled to improve the forming quality of the polyester drawn yarn;

[0070] The spindle shaft length is 1600mm, the number of silk cakes arranged on the spindle shaft is 12; the silk cake winding diameter is 378mm;

[0071] The friction roller corresponds to the spindle shaft one by one, and the friction roller is located directly above the spindle shaft, and the length of the friction roller and the spindle shaft are equal; the diameter of the friction roller is 85mm; along the axial direction, the friction roller corresponding to each silk cake is divided into three areas: left, middle and right, with the middle area accounting for 56%, and the left and right areas accounting for 22% respectively; the surface roughness Ra of the friction roller in the middle area is 0.7μm;

[0072] The left and right areas of the friction roller corresponding to each silk cake are equally divided into four small areas. The roughness Ra of the four small areas from right to left in the left area are 0.5μm, 0.3μm, 0.15μm, and 0.08μm respectively, and the roughness Ra of the four small areas from left to right in the right area are 0.5μm, 0.3μm, 0.15μm, and 0.08μm respectively.

[0073] Let one end of the spindle shaft for loading the paper tube be end face a, and the other end be end face b. Establish a spatial rectangular coordinate system with the straight line passing through end face a and parallel to the horizontal plane as the X-axis, the straight line passing through end face a and perpendicular to the horizontal plane as the Y-axis, and the straight line parallel to the center axis of the spindle shaft as the Z-axis. The end of the friction roller close to end face a is offset upward by 0.09 mm along the Y-axis direction and by 0.08 mm along the X-axis direction.

[0074] The downgrade rate of brake marks on wound silk cakes is 0.07%.

[0075] Example 5

[0076] A method for improving the forming quality of polyester drawn yarn, the specific process is as follows:

[0077] In the winding process of polyester drawn yarn for warp knitting, the surface roughness of the friction roller and the relative position between the friction roller and the spindle are controlled to improve the forming quality of the polyester drawn yarn;

[0078] The spindle shaft length is 1800mm, the number of silk cakes arranged on the spindle shaft is 16; the silk cake winding diameter is 380mm;

[0079] The friction roller corresponds to the spindle shaft one by one, and the friction roller is located directly above the spindle shaft, and the length of the friction roller is equal to that of the spindle shaft; the diameter of the friction roller is 85.5 mm; along the axial direction, the friction roller corresponding to each silk cake is divided into three areas: left, middle, and right, with the middle area accounting for 55%, and the left and right areas accounting for 22.5% respectively; the surface roughness Ra of the friction roller in the middle area is 0.6 μm;

[0080] The left and right areas of the friction roller corresponding to each silk cake are equally divided into four small areas. The roughness Ra of the four small areas from right to left in the left area are 0.4μm, 0.3μm, 0.2μm, and 0.1μm respectively, and the roughness Ra of the four small areas from left to right in the right area are 0.4μm, 0.3μm, 0.2μm, and 0.1μm respectively.

[0081] Let one end of the spindle shaft for loading the paper tube be end face a, and the other end be end face b. Establish a spatial rectangular coordinate system with the straight line passing through end face a and parallel to the horizontal plane as the X-axis, the straight line passing through end face a and perpendicular to the horizontal plane as the Y-axis, and the straight line parallel to the center axis of the spindle shaft as the Z-axis. The end of the friction roller close to end face a is offset upward by 0.1 mm along the Y-axis direction and by 0.09 mm along the X-axis direction.

[0082] The downgrade rate of brake marks on wound silk cakes is 0.09%.

Claims

1. A method for improving the molding quality of polyester drawn yarn, characterized in that: In the winding process of polyester drawn yarn for warp knitting, the surface roughness of the friction roller and the relative position between the friction roller and the spindle are controlled to improve the forming quality of the polyester drawn yarn; Along the axial direction, the friction roller corresponding to each silk cake is divided into three areas: left, middle and right. The middle area accounts for 55-60%, and the left and right areas account for 20-22.5% respectively. The roughness Ra of the friction roller surface in the middle area is 0.8±0.2μm. From the middle area to the left and right areas, the roughness Ra of the friction roller surface gradually decreases to 0.1±0.02μm. Let the end of the spindle shaft for loading the paper tube be end face a, and establish a spatial rectangular coordinate system with the straight line passing through end face a and parallel to the horizontal plane as the X-axis, the straight line passing through end face a and perpendicular to the horizontal plane as the Y-axis, and the straight line parallel to the center axis of the spindle shaft as the Z-axis. The end of the friction roller close to end face a is offset upward by 0.07~0.1mm along the Y-axis direction, and the offset along the X-axis direction is less than or equal to 0.09mm.

2. A method for improving the forming quality of polyester drawn yarn according to claim 1, characterized in that: The left and right areas of the friction roller corresponding to each silk cake are equally divided into four small areas. The roughness Ra of the four small areas in the left area from right to left are 0.6±0.2μm, 0.4±0.1μm, 0.2±0.05μm, and 0.1±0.02μm, respectively. The roughness Ra of the four small areas in the right area from left to right are 0.6±0.2μm, 0.4±0.1μm, 0.2±0.05μm, and 0.1±0.02μm, respectively.

3. A method for improving the forming quality of polyester drawn yarn according to claim 1, characterized in that: The spindle shaft length is 1150~1800mm.

4. A method for improving the forming quality of polyester drawn yarn according to claim 3, characterized in that: The number of silk cakes arranged on the spindle shaft is 8 to 16.

5. The method for improving the forming quality of polyester drawn yarn according to claim 1, characterized in that: The diameter of the silk cake roll ranges from 360 to 380 mm.

6. A method for improving the forming quality of polyester drawn yarn according to claim 1, characterized in that: The length of the friction roller is equal to that of the spindle shaft, and the diameter of the friction roller is 84.5~85.5mm.

7. A method for improving the forming quality of polyester drawn yarn according to claim 1, characterized in that: The downgrade rate of brake marks on the wound silk cake is ≤0.1%.

Citation Information

Patent Citations

  • Take-off and drawing godet units in production line for fully drawn yarn melt spun multifilaments

    DE19909073A1

  • Device for producing a thread reserve and / or an end ridge of thread

    EP1125879A2

  • High friction roller and manufacture thereof

    JP1991095062A

  • Drawing of monofilament for screen gauze

    JP1994033334A

  • Method for direct spun yarn drawing of polyester fiber

    JP2004277892A