Method for recycling battery positive electrode material from sludge
After organic reducing acid leaching and pH adjustment of the sludge incineration ash, Li, Fe, Mn and carbon sources were added for hydrothermal synthesis, the problem of long process flow in the existing technology was solved and the positive electrode material of the battery was realized. Efficient preparation and material performance improvement.
Patent Information
- Application Number
- CN202411205132.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-30
AI Technical Summary
In the prior art, the process flow of recovering battery positive electrode materials from sludge is relatively long, and a shortening method is needed.
By incineration of the dried sludge and leaching with organic reducing acid, the phosphorus-containing supernatant was obtained and pH was adjusted. Li source, Fe source, Mn source, template agent and carbon source were added to carry out hydrothermal heat Synthesis is made to prepare the battery positive electrode material.
The process flow for preparing the positive electrode material of the battery is shortened, the leaching efficiency of phosphorus elements and the carbon coating effect are improved, and the conductivity and ion conduction ability of the material are improved.
Smart Images

Figure CN119079965A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sludge resource utilization, and in particular to a method for recovering battery positive electrode materials from sludge. Background Art
[0002] Pollutants and nutrients in sewage are aggregated by the proliferation of bacteria and chemical agents, eventually forming sludge. With the rapid development of new energy vehicles, energy storage batteries and other industries, the output of positive electrode materials (such as lithium iron manganese phosphate) is also rising, resulting in an increase in the demand for its production raw materials (such as phosphorus).
[0003] In the related art, the method for recovering phosphorus from sludge and preparing battery positive electrode materials mainly adopts a multi-stage synthesis method, but the process flow of this method is relatively long.
[0004] Therefore, there is an urgent need for a method for recovering battery positive electrode materials from sludge to solve this technical problem. Summary of the invention
[0005] The invention provides a method for recovering battery positive electrode materials from sludge, which can shorten the process flow of preparing battery positive electrode materials.
[0006] The present invention provides a method for recovering battery positive electrode materials from sludge, comprising:
[0007] Incinerating the dried sludge to obtain sludge incineration ash;
[0008] Leaching the sludge incineration ash with an organic reducing acid, and obtaining a phosphorus-containing supernatant after solid-liquid separation;
[0009] Adjusting the pH of the phosphorus-containing supernatant, and adding a Li source, an Fe source, a Mn source, a template agent and a carbon source to the phosphorus-containing supernatant after the pH adjustment to obtain a mixed solution;
[0010] The mixed solution is subjected to hydrothermal synthesis to obtain a positive electrode material for a battery.
[0011] As can be seen from the above scheme, the present invention provides a method for recovering positive electrode materials from sludge, by incinerating the dried sludge to obtain sludge incineration ash, then leaching the sludge incineration ash with an organic reducing acid, and obtaining a phosphorus-containing supernatant after solid-liquid separation, then adjusting the pH of the phosphorus-containing supernatant, and adding a Li source, an Fe source, a Mn source, a template and a carbon source to the phosphorus-containing supernatant after pH adjustment to obtain a mixed solution, and hydrothermally synthesizing the mixed solution to obtain a positive electrode material for the battery. Therefore, the above technical scheme is a hydrothermal synthesis treatment directly performed on the mixed solution after pH adjustment, so the process flow of preparing the positive electrode material for the battery can be shortened. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0013] Figure 1 A schematic diagram of a method for recovering battery positive electrode materials from sludge provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0014] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0015] See also Figure 1 One embodiment of the present invention provides a method for recovering positive electrode materials from sludge, the method comprising:
[0016] Step 100, incinerating the dried sludge to obtain sludge incineration ash;
[0017] Step 102: leaching the sludge incineration ash with an organic reducing acid, and obtaining a phosphorus-containing supernatant after solid-liquid separation;
[0018] Step 104, adjusting the pH of the phosphorus-containing supernatant, and adding a Li source, an Fe source, a Mn source, a template agent and a carbon source to the phosphorus-containing supernatant after the pH adjustment to obtain a mixed solution;
[0019] Step 106: Perform hydrothermal synthesis on the mixed solution to obtain a positive electrode material for a battery.
[0020] In this embodiment, the dried sludge is incinerated to obtain sludge incineration ash, and then the sludge incineration ash is leached with an organic reducing acid, and a phosphorus-containing supernatant is obtained after solid-liquid separation, and then the pH of the phosphorus-containing supernatant is adjusted, and a Li source, an Fe source, a Mn source, a template agent and a carbon source are added to the phosphorus-containing supernatant after pH adjustment to obtain a mixed solution, and finally the mixed solution is hydrothermally synthesized to obtain a battery positive electrode material. Therefore, the above technical scheme is a hydrothermal synthesis treatment directly performed on the mixed solution after pH adjustment, so the process flow of preparing the battery positive electrode material can be shortened.
[0021] In some embodiments, the incineration temperature is 750-900° C. to ensure the incineration effect of the dried sludge.
[0022] In one embodiment of the present invention, the organic reducing acid includes at least one of oxalic acid, ascorbic acid, citric acid, formic acid, glyoxylic acid and salicylic acid.
[0023] In some embodiments, the solid-liquid ratio of the sludge incineration ash to the organic reducing acid can be 1:50 to 1:200, the leaching time can be 2 to 4 hours, and the tumbling oscillation rate can be 60 to 120 rpm to ensure that the organic reducing acid can effectively extract phosphorus from the sludge incineration ash.
[0024] In this embodiment, the organic reducing acid can make the phosphorus element in the sludge incineration ash more leached out, and at the same time, the reducing property of the organic reducing acid can be used to prevent the divalent iron salts in the sludge incineration ash and the divalent iron in the battery positive electrode material from being oxidized to trivalent iron.
[0025] In the related art, some leaching solutions usually use high-concentration inorganic acids such as sulfuric acid and nitric acid to utilize their high acidity to leach phosphorus. However, the preparation of battery positive electrode materials requires a neutral environment, so other reagents need to be added later to achieve the neutralization effect. Therefore, this method consumes a lot of reagents. However, the organic reducing acid in this embodiment can not only provide an acidic environment to leach phosphorus, but also utilize the reducing property of the organic reducing acid and the chelating property of the organic acid radical to provide additional driving force for the leaching of phosphorus in sludge incineration ash.
[0026] In addition, Fe / Al-bound phosphorus (usually FePO 4 、AlPO 4 ) is a phosphorus form that occupies a considerable part of the sludge incineration ash. Organic reducing acids can convert insoluble FePO 4 The process can be summarized as "reductive dissolution". 2 O 4 2- , Citrate also has a strong chelating and coordination ability, which can convert AlPO 4 The Al element in the precipitate is replaced by chelation to form Al - Organic acid radical ligands release phosphorus into the liquid phase. This process can be summarized as "coordinated dissolution". Under the combined effect of "acidic-reducing-chelating properties", the use of organic reducing acids can show better phosphorus leaching effects than inorganic acids, and can leach more phosphorus at lower concentrations.
[0027] In one embodiment of the present invention, the concentration of the organic reducing acid is 0.04-0.5 mol / L. At this concentration, the leaching effect of the organic reducing acid on phosphorus element can be guaranteed.
[0028] In one embodiment of the present invention, the pH of the phosphorus-containing supernatant is adjusted using aqueous ammonia.
[0029] In this embodiment, by adding ammonia water to the phosphorus-containing supernatant, the effect of not introducing impurities during the pH adjustment process can be achieved. This is because ammonia water will produce ammonia gas and be discharged during the subsequent hydrothermal synthesis treatment.
[0030] In one embodiment of the present invention, the pH of the phosphorus-containing supernatant after pH adjustment is 5-8.
[0031] In this embodiment, the pH of the phosphorus-containing supernatant is adjusted to 5-8, which not only helps to remove the Fe(III) / Al / Ca / Mg / heavy metal impurities that are simultaneously precipitated during the hydrothermal synthesis treatment, but also retains the soluble metal ions (such as Na + , K + ).
[0032] Usually, the positive electrode material of the battery needs to be further carbon-coated before it can be used. In the related technology, the commonly used carbon-coating methods are hydrothermal method and heating calcination method. The former is to add a carbon source simultaneously during the Li supplementation process. Although the carbon-coated positive electrode material can be directly obtained, the carbon adhesion effect is limited; the latter is to place the battery-grade positive electrode material and the carbon source in a high-temperature reducing gas environment for calcination after Li supplementation. Although this method can improve the carbon-coating effect to a certain extent, the distributed steps further lengthen the processing flow, and the carbon coating uniformity is not as good as the hydrothermal method.
[0033] However, in this embodiment, the soluble metal salt (i.e., the retained sodium salt and potassium salt) can enhance the reactivity of -OH, -COOH, and -COC- bonds on the carbon source by bridging, changing the charge density, or directly catalyzing the reaction, thereby promoting deoxygenation polymerization, decarboxylation polymerization, and aromatization between carbon sources, as well as condensation polymerization within the carbon source. The enhancement of these reactions greatly improves the carbon coating degree on the surface of the battery positive electrode material compared to the traditional hydrothermal process, and improves the conductivity and ion conductivity of the battery positive electrode material.
[0034] In some embodiments, the adjusted solution is stirred at a speed of 1 to 200 rpm and a stirring time of 10 to 240 min to allow the adjusted solution to be fully mixed.
[0035] In some embodiments, the phosphorus-containing supernatant after pH adjustment can be filtered using a 0.22 μm filter head to remove the precipitate, so as to remove the solid particles that have not been separated.
[0036] In one embodiment of the present invention, the phosphorus-containing supernatant is used for cyclic leaching of new sludge incineration ash.
[0037] In this embodiment, the phosphorus-containing supernatant is recycled for cyclic leaching of phosphorus in sludge incineration ash, thereby reducing reagent consumption.
[0038] In one embodiment of the present invention, the reaction temperature of the hydrothermal synthesis is 120-250° C., and the reaction time is 1-24 hours.
[0039] In one embodiment of the present invention, the Li source includes LiOH, LiCl, Li 2 CO 3 and Li 2 SO 4 At least one of .
[0040] In one embodiment of the present invention, the Fe source includes FeSO 4 、FeCl 2 、Fe(NO 3 ) 2 and FeC 2 O 4 At least one of .
[0041] In one embodiment of the present invention, the Mn source includes MnSO 4 、MnCl 2 、Mn(NO 3 ) 2 and MnC 2 O 4 At least one of .
[0042] In one embodiment of the present invention, the template agent includes at least one of polyvinyl alcohol, ethylene glycol, hexadecyltrimethylammonium bromide and sodium dodecylbenzene sulfonate.
[0043] In one embodiment of the present invention, the carbon source includes at least one of sucrose, glucose, furfuryl alcohol, starch, graphene, carbon nanotubes, carbon black and acetylene black.
[0044] In this embodiment, when the Li source is a soluble lithium salt and its hydrate, the Fe source is a soluble iron salt and its hydrate, and the Mn source is a soluble manganese salt and its hydrate, the mixed solution can have higher ionic conductivity, better thermal stability and better electrochemical stability.
[0045] In this embodiment, the template forms steric hindrance between the battery positive electrode material particles through coordination during the hydrothermal synthesis process to prevent the battery positive electrode material particles from being too large or sticking together, thereby playing a role in regulating the size and uniformity of the battery positive electrode material particles.
[0046] In this embodiment, during the hydrothermal synthesis process, the carbon source generates a carbon-rich structure through a polymerization reaction between organic matter, and is attached to the surface of the battery positive electrode material through a bonding reaction between the surfaces of organic-inorganic materials, ultimately forming a dense carbon layer to increase the conductivity of the battery positive electrode material and the Li ion transfer efficiency.
[0047] In one embodiment of the present invention, when the Fe source is an inorganic acid radical iron salt and the Mn source is an inorganic acid radical manganese salt, the molar ratio of the P element in the Li source, the Fe source, the Mn source and the phosphorus-containing supernatant is 3:x:(1-x):1, where x is greater than 0 and less than 1.
[0048] In one embodiment of the present invention, when the Fe source is an organic acid iron salt and the Mn source is an organic acid manganese salt, the molar ratio of the P element in the Li source, the Fe source, the Mn source and the phosphorus-containing supernatant is 1:x:(1-x):1, where x is greater than 0 and less than 1.
[0049] In one embodiment of the present invention, the dosage of the carbon source is 1-10% of the total mass of the positive electrode material of the battery.
[0050] In one embodiment of the present invention, the dosage of the template agent is 1-25% of the total mass of the battery positive electrode material.
[0051] In some embodiments, the total mass is the theoretical yield of the positive electrode material of the battery, calculated by the following formula:
[0052] Total mass = (157 + x) * moles of phosphorus in the liquid phase.
[0053] In one embodiment of the present invention, step 106 may specifically include:
[0054] Performing hydrothermal synthesis on the mixed solution to obtain a hydrothermal synthesis product;
[0055] Performing solid-liquid separation on the hydrothermal synthesis product to obtain a solid product;
[0056] The solid product is washed alternately with deionized water and an ethanol solution, and the washed solid product is freeze-dried;
[0057] The freeze-dried solid product is roasted under an inert atmosphere to obtain a positive electrode material for a battery.
[0058] In this embodiment, a vacuum filtration method can be used to separate the solid and liquid of the hydrothermal synthesis product, so that the solid and liquid of the hydrothermal synthesis product can be better separated.
[0059] Among them, alternating washing can remove impurity ions in the solid product, and freeze-drying the washed solid product can remove moisture in the solid product.
[0060] In some embodiments, the calcination temperature may be 500-800° C., so that the freeze-dried solid product can be fully calcined, thereby obtaining a positive electrode material for a battery.
[0061] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for recovering positive electrode materials from sludge, characterized in that: include: Incinerating the dried sludge to obtain sludge incineration ash; Leaching the sludge incineration ash with an organic reducing acid, and obtaining a phosphorus-containing supernatant after solid-liquid separation; Adjusting the pH of the phosphorus-containing supernatant, and adding a Li source, an Fe source, a Mn source, a template agent and a carbon source to the phosphorus-containing supernatant after the pH adjustment to obtain a mixed solution; The mixed solution is subjected to hydrothermal synthesis to obtain a positive electrode material for a battery.
2. The method according to claim 1, characterized in that The organic reducing acid includes at least one of oxalic acid, ascorbic acid, citric acid, formic acid, glyoxylic acid and salicylic acid.
3. The method according to claim 1, characterized in that: The concentration of the organic reducing acid is 0.04-0.5 mol / L.
4. The method according to claim 1, characterized in that The pH of the phosphorus-containing supernatant is adjusted using aqueous ammonia.
5. The method according to claim 1, characterized in that The pH of the phosphorus-containing supernatant after pH adjustment is 5-8.
6. The method according to claim 1, characterized in that The phosphorus-containing supernatant is used for cyclic leaching of new sludge incineration ash.
7. The method according to claim 1, characterized in that The reaction temperature of the hydrothermal synthesis is 120-250° C., and the reaction time is 0-24 hours.
8. The method according to claim 1, characterized in that The Li source includes at least one of LiOH, LiCl, Li2CO3 and Li2SO4; and / or, The Fe source includes at least one of FeSO4, FeCl2, Fe(NO3)2 and FeC2O4; and / or, The Mn source includes at least one of MnSO4, MnCl2, Mn(NO3)2 and MnC2O4; and / or, The template agent comprises at least one of polyvinyl alcohol, ethylene glycol, hexadecyltrimethylammonium bromide and sodium dodecylbenzene sulfonate; and / or, The carbon source includes at least one of sucrose, glucose, furfuryl alcohol, starch, graphene, carbon nanotubes, carbon black and acetylene black.
9. The method according to claim 1, characterized in that: When the Fe source is an inorganic acid radical iron salt and the Mn source is an inorganic acid radical manganese salt, the molar ratio of the Li source, the Fe source, the Mn source and the P element in the phosphorus-containing supernatant is 3:x:(1-x):1, where x is greater than 0 and less than 1; and / or, When the Fe source is an organic acid radical iron salt and the Mn source is an organic acid radical manganese salt, the molar ratio of the Li source, the Fe source, the Mn source and the P element in the phosphorus-containing supernatant is 1:x:(1-x):1, where x is greater than 0 and less than 1; and / or, The dosage of the carbon source is 1 to 10% of the total mass of the battery positive electrode material; The dosage of the template agent is 1-25% of the total mass of the battery positive electrode material.
10. The method according to any one of claims 1 to 9, characterized in that The step of subjecting the mixed solution to hydrothermal synthesis to obtain a positive electrode material for a battery comprises: Performing hydrothermal synthesis on the mixed solution to obtain a hydrothermal synthesis product; Performing solid-liquid separation on the hydrothermal synthesis product to obtain a solid product; Washing the solid product alternately with deionized water and ethanol solution, and freeze-drying the washed solid product; The freeze-dried solid product is roasted under an inert atmosphere to obtain a positive electrode material for a battery.
Citation Information
Patent Citations
Method for preparing iron phosphate from municipal sludge incineration ash and battery-grade iron phosphate
CN113401887A
Method for separating heavy metals and recovering phosphorus and iron from sludge incineration ash
CN114427033A
Method for recovering phosphorus from incineration ash of organic material and method for producing fertilizer
JP2010132465A
Sewage sludge incineration ash processing method
JP2014163841A