Sodium ferric phosphate positive electrode material and preparation method thereof, positive electrode plate and sodium ion battery

The preparation of sodium iron phosphate positive electrode material under a protective atmosphere by co-precipitation reaction method has solved the problems of high energy consumption and complex process of the existing NaFePO4 preparation method, achieved high performance and low cost preparation, and improved the electricity of sodium ion batteries Chemical properties.

CN119079969APending Publication Date: 2024-12-06SUZHOU TETRAHEDRON NEW ENERGY TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411265039.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing NaFePO4 preparation method has high energy consumption, complex process and high equipment requirements, making it difficult to achieve a preparation method with good product performance, simple process, energy-saving and environmentally friendly and high safety performance.

Method used

By using the co-precipitation reaction method, the co-precipitation reaction between the phosphorus source and the iron source was carried out for 4h to 10h at 95°C~160°C under a protective atmosphere, the pH value was adjusted to 4~8, and the positive electrode material of sodium iron phosphate was prepared, which simplified the Process flow to reduce energy consumption and environmental pollution.

Benefits of technology

The high purity, good crystallinity and small average particle size of sodium iron phosphate cathode material are achieved, and the gram capacity, rate performance and low temperature performance of sodium ion batteries are improved, and the process is simple and safety performance is high.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079969A_ABST
    Figure CN119079969A_ABST
Patent Text Reader

Abstract

The invention relates to a sodium ferric phosphate positive electrode material and a preparation method thereof, a positive electrode plate and a sodium ion battery, the preparation method of the sodium ferric phosphate positive electrode material comprises the following steps: mixing a phosphorus source and a first solvent, and adjusting the pH value of the obtained first mixed solution to 4-8; adding a solution containing a sodium source and a solution containing an iron source into the first mixed solution at the same time, and adjusting the pH value of the obtained second mixed solution to be the same as the pH value of the first mixed solution; the second mixed solution is subjected to a co-precipitation reaction under the protective atmosphere condition, the technological conditions of the co-precipitation reaction include that the reaction temperature is 95-160 DEG C, the reaction time is 4-10 h, and the sodium ferric phosphate positive electrode material is prepared; the preparation method of the sodium iron phosphate positive electrode material is simple in process, energy-saving, environment-friendly and high in safety performance, the prepared sodium iron phosphate positive electrode material is applied to a sodium ion battery, and the gram volume, the rate capability and the low-temperature performance of the battery can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of positive electrode materials, and in particular to a sodium iron phosphate positive electrode material and a preparation method thereof, a positive electrode sheet and a sodium ion battery. Background Art

[0002] Lithium-ion batteries (LIBs) have the advantages of high energy density and long cycle life, and have been widely used in portable electronic devices and electric vehicles. In recent years, with the development of electric vehicles, the resource reserves of lithium are limited, the price continues to rise, and the cost is getting higher and higher. Sodium-ion batteries (SIBs) have the characteristics of high safety, great application potential, abundant reserves, and low cost, so they have received widespread attention. Polyanionic compounds have the advantages of stable structure and small volume change during charge and discharge. Sodium iron phosphate (NaFePO4) crystals have a high theoretical capacity (155mAh·g -1 ) and has become a promising cathode material for sodium-ion batteries. + The radius ratio Li + The large radius makes the structure of the active material easily destroyed during the charge / discharge process.

[0003] At present, the preparation methods of NaFePO4 include traditional solid phase method, hydrothermal / solvothermal synthesis method, ion exchange method, etc. The traditional solid phase method has high energy consumption, large synthetic particles, and difficult to control morphology. The hydrothermal / solvothermal synthesis method has high requirements for production equipment. The ion exchange method needs to exchange Li in LiFePO4 for Na, and the process is relatively complicated. Therefore, it is urgent to develop a preparation method of NaFePO4 with good product performance, simple process, energy saving and environmental protection, and high safety performance. Summary of the invention

[0004] The present application provides a sodium iron phosphate positive electrode material and a preparation method thereof, a positive electrode plate and a sodium ion battery. The preparation method of the sodium iron phosphate positive electrode material has a simple process, energy saving, environmental protection and high safety performance. The prepared sodium iron phosphate positive electrode material is applied to sodium ion batteries to improve the battery's gram capacity, rate performance and low temperature performance.

[0005] In a first aspect of the present application, a method for preparing a sodium iron phosphate positive electrode material is provided, comprising the following steps:

[0006] Mixing the phosphorus source and the first solvent, and adjusting the pH value of the obtained first mixed solution to 4-8;

[0007] Adding a solution containing a sodium source and a solution containing an iron source to the first mixed solution at the same time, and adjusting the pH value of the obtained second mixed solution to be the same as the pH value of the first mixed solution;

[0008] The second mixed solution is subjected to a coprecipitation reaction under protective atmosphere conditions, wherein the process conditions of the coprecipitation reaction include: a reaction temperature of 95° C. to 160° C., and a reaction time of 4 h to 10 h, to prepare the sodium iron phosphate positive electrode material (NaFePO 4 ).

[0009] In some embodiments, the process conditions of the coprecipitation reaction also include: a pressure of 0.1 MPa to 0.4 MPa.

[0010] In some embodiments, before the step of simultaneously adding the solution containing the sodium source and the solution containing the iron source to the first mixed solution, the step further includes: heating the first mixed solution to a temperature of 95° C. to 160° C.

[0011] In some embodiments, the step of mixing the phosphorus source and the first solvent and adjusting the pH value of the obtained first mixed solution to 4-8 includes: using a first pH adjuster to adjust the pH value of the first mixed solution to 4-8.

[0012] In some embodiments, a solution containing a sodium source and a solution containing an iron source are simultaneously added to the first mixed solution, and the step of adjusting the pH value of the obtained second mixed solution to be the same as the pH value of the first mixed solution includes: using a second pH adjuster to adjust the pH value of the second mixed solution to 4-8.

[0013] In some embodiments, the first pH adjuster and the second pH adjuster each independently include one or more of phosphoric acid, acetic acid, citric acid, sulfuric acid, and sodium hydroxide.

[0014] In some embodiments, the concentration of the first mixed solution is 0.1 mol / L to 1 mol / L.

[0015] In some embodiments, the concentration of the solution containing the sodium source is 0.1 mol / L to 1 mol / L.

[0016] In some embodiments, the concentration of the solution containing the iron source is 0.1 mol / L to 1 mol / L.

[0017] In some embodiments, the phosphorus source includes one or more of sodium dihydrogen phosphate, ammonium dihydrogen phosphate, sodium phosphate, potassium dihydrogen phosphate, and phosphoric acid.

[0018] In some embodiments, the sodium source includes one or more of sodium dihydrogen phosphate, sodium sulfate, sodium phosphate, sodium acetate, and sodium chloride.

[0019] In some embodiments, the iron source includes one or more of ferrous sulfate, ferrous chloride, and ferric acetate.

[0020] In some embodiments, the solution containing the sodium source contains a second solvent, the solution containing the iron source contains a third solvent, and the first solvent, the second solvent, and the third solvent each independently include one or more of water and alcohol solvents.

[0021] In some embodiments, after the step of subjecting the second mixed solution to a co-precipitation reaction under protective atmosphere conditions, the method further includes: separating the obtained product, and sequentially washing and drying the obtained precipitate to obtain the sodium iron phosphate positive electrode material.

[0022] The second aspect of the present application provides a sodium iron phosphate positive electrode material, which is prepared using the preparation method described in the first aspect of the present application.

[0023] In some embodiments, the average particle size of the sodium iron phosphate positive electrode material is 50 nm to 150 nm.

[0024] In some embodiments, the purity of the sodium iron phosphate positive electrode material is 98% to 99.99%.

[0025] The third aspect of the present application provides a positive electrode plate, comprising the sodium iron phosphate positive electrode material described in the second aspect of the present application.

[0026] In a fourth aspect of the present application, a sodium ion battery is provided, comprising at least one of the sodium iron phosphate positive electrode material described in the second aspect of the present application and the positive electrode sheet described in the third aspect of the present application.

[0027] The fifth aspect of the present application provides an electrical device comprising the sodium ion battery described in the fourth aspect of the present application.

[0028] Compared with the traditional technology, the preparation method of the sodium iron phosphate positive electrode material has at least the following advantages:

[0029] (1) The preparation method has simple steps, is easy to implement, and is suitable for large-scale industrial production; the temperature of the coprecipitation reaction in the preparation method is relatively low, which greatly reduces energy consumption and environmental pollution compared with the traditional solid phase method; compared with the hydrothermal / solvothermal synthesis method, the preparation method has lower requirements on production equipment and reduces production costs; compared with the ion exchange method, the preparation method does not need to exchange Li in LiFePO4 for Na, simplifies the process flow, avoids the use of a large amount of organic solvents, and is more environmentally friendly; the preparation method is carried out at low temperature and low pressure, which reduces safety risks and has higher safety performance than the hydrothermal / solvothermal synthesis method that needs to be carried out at high temperature and high pressure.

[0030] (2) In the above preparation method, by controlling the pH value of the first mixed solution and the second mixed solution to be 4-8, the solubility of the phosphorus source, the sodium source and the iron source in the solution and the stability of the pH environment of the solution system can be improved, which is conducive to the full co-precipitation reaction of the three. Adding the solution containing the sodium source and the solution containing the iron source to the first mixed solution at the same time can make the concentration, equivalent and pH environment of the reactants relatively stable, and at the same time can reduce the oxidation of ferrous ions and the generation of impurities, thereby improving the purity of the sodium iron phosphate positive electrode material. The sodium iron phosphate positive electrode material obtained by the preparation method has better crystallinity and smaller average particle size, which can improve the electrochemical performance of the sodium ion battery containing the sodium iron phosphate positive electrode material, such as gram capacity, rate performance, low temperature performance and cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the XRD (X-ray diffraction) pattern of the sodium iron phosphate positive electrode material prepared in Example 1 of the present application. DETAILED DESCRIPTION

[0032] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0033] In this application, "first aspect", "second aspect", "third aspect", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0034] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.

[0035] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0036] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0037] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by technicians in the technical field of this application. The terms used in this application and in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this application includes any and all combinations of one or more related listed items. The term "multiple" in this application means at least two, such as two, three, etc., unless otherwise clearly and specifically limited.

[0038] An embodiment of the present application provides a method for preparing a sodium iron phosphate positive electrode material, comprising the following steps:

[0039] Mixing the phosphorus source and the first solvent, and adjusting the pH value of the obtained first mixed solution to 4-8;

[0040] Adding a solution containing a sodium source and a solution containing an iron source to the first mixed solution at the same time, and adjusting the pH value of the obtained second mixed solution to be the same as the pH value of the first mixed solution;

[0041] The second mixed solution is subjected to a coprecipitation reaction under protective atmosphere conditions. The process conditions of the coprecipitation reaction include: a reaction temperature of 95° C. to 160° C. and a reaction time of 4 h to 10 h to prepare a sodium iron phosphate positive electrode material.

[0042] The preparation method has simple steps, is easy to implement, and is suitable for large-scale industrial production; the temperature of the coprecipitation reaction in the preparation method is relatively low, which greatly reduces energy consumption and environmental pollution compared with the traditional solid phase method; compared with the hydrothermal / solvothermal synthesis method, the preparation method has lower requirements on production equipment and reduces production costs; compared with the ion exchange method, the preparation method does not need to exchange Li in LiFePO4 for Na, simplifies the process flow, avoids the use of a large amount of organic solvents, and is more environmentally friendly; the preparation method is carried out at low temperature and low pressure, which reduces safety risks and has higher safety performance compared with the hydrothermal / solvothermal synthesis method that needs to be carried out at high temperature and high pressure;

[0043] In the above preparation method, by controlling the pH value of the first mixed solution and the second mixed solution to be 4-8, the solubility of the phosphorus source, sodium source and iron source in the solution and the stability of the pH environment of the solution system can be improved, which is conducive to the full co-precipitation reaction of the three. Adding a solution containing a sodium source and a solution containing an iron source to the first mixed solution at the same time can make the concentration, equivalent and pH environment of the reactants relatively stable, and at the same time can reduce the oxidation of ferrous ions and the generation of impurities, thereby improving the purity of the sodium iron phosphate positive electrode material. The sodium iron phosphate positive electrode material obtained by the preparation method has better crystallinity and a smaller average particle size, which can improve the electrochemical performance of the sodium ion battery containing the sodium iron phosphate positive electrode material, such as gram capacity, rate performance, low temperature performance and cycle stability. In summary, the above preparation method has the advantages of excellent product performance, simple process, energy saving and environmental protection, high safety performance, etc., and is an ideal preparation method for sodium iron phosphate positive electrode material. Specifically, the pH value of the first mixed solution includes but is not limited to: 4, 5, 6, 7, 8 or a range between any two of the foregoing, the pH value of the second mixed solution includes but is not limited to: 4, 5, 6, 7, 8 or a range between any two of the foregoing, the reaction temperature includes but is not limited to: 95°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C or a range between any two of the foregoing, and the reaction time includes but is not limited to: 4h, 5h, 6h, 7h, 8h, 9h, 10h or a range between any two of the foregoing.

[0044] When the pH value of the first mixed solution is too low, the yield of the sodium iron phosphate positive electrode material is relatively low; when the pH value of the first mixed solution is too high, the average particle size of the sodium iron phosphate positive electrode material is relatively large and there are more impurities, which affects the battery's gram capacity, rate performance and low temperature performance.

[0045] In some embodiments, the pressure of the coprecipitation reaction is 0.1 MPa to 0.4 MPa. The pressure of the coprecipitation reaction in the above preparation method is lower than that of the hydrothermal / solvothermal synthesis method, so the safety performance is higher.

[0046] In some embodiments, before the step of simultaneously adding a solution containing a sodium source and a solution containing an iron source to the first mixed solution, it also includes: heating the first mixed solution so that the temperature of the first mixed solution is 95°C to 160°C. Such a design can improve the solubility of the phosphorus source, sodium source and iron source, shorten the time for heating during the coprecipitation reaction, reduce the generation of impurities during the heating process, and be more conducive to the improvement of the sodium iron phosphate positive electrode material. Specifically, the temperature of the first mixed solution includes but is not limited to: 95°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C or a range between any two of the foregoing.

[0047] In some embodiments, the step of mixing the phosphorus source and the first solvent and adjusting the pH value of the obtained first mixed solution to 4-8 includes: using a first pH adjuster to adjust the pH value of the first mixed solution to 4-8.

[0048] In some embodiments, a solution containing a sodium source and a solution containing an iron source are simultaneously added to the first mixed solution, and the step of adjusting the pH value of the obtained second mixed solution to be the same as the pH value of the first mixed solution comprises: using a second pH adjuster to adjust the pH value of the second mixed solution to 4-8.

[0049] In some embodiments, the first pH adjuster and the second pH adjuster each independently include one or more of phosphoric acid, acetic acid, citric acid, sulfuric acid, and sodium hydroxide.

[0050] In some embodiments, the protective atmosphere includes at least one of a nitrogen atmosphere, a helium atmosphere, a neon atmosphere, and an argon atmosphere.

[0051] In some embodiments, the concentration of the first mixed solution is 0.1 mol / L to 1 mol / L. Specifically, the above concentration includes but is not limited to: 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L or a range between any two of the foregoing.

[0052] In some embodiments, the concentration of the solution containing the sodium source is 0.1 mol / L to 1 mol / L. Specifically, the above concentration includes but is not limited to: 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L or a range between any two of the foregoing.

[0053] In some embodiments, the concentration of the solution containing the iron source is 0.1 mol / L to 1 mol / L. Specifically, the above concentration includes but is not limited to: 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L or a range between any two of the foregoing.

[0054] In some embodiments, the phosphorus source includes one or more of sodium dihydrogen phosphate, ammonium dihydrogen phosphate, sodium phosphate, potassium dihydrogen phosphate, and phosphoric acid.

[0055] In some embodiments, the sodium source includes one or more of sodium dihydrogen phosphate, sodium sulfate, sodium phosphate, sodium acetate, and sodium chloride.

[0056] In some embodiments, the iron source includes one or more of ferrous sulfate, ferrous chloride, and ferric acetate.

[0057] In some embodiments, the solution comprising the sodium source comprises the second solvent, the solution comprising the iron source comprises the third solvent, and the first solvent, the second solvent and the third solvent each independently comprise one or more of water and an alcoholic solvent. In some embodiments, the alcoholic solvent comprises one or more of methanol, ethanol, glycerol and ethylene glycol. Optionally, the first solvent, the second solvent and the third solvent are all water.

[0058] In some embodiments, after the step of subjecting the second mixed solution to a co-precipitation reaction under protective atmosphere conditions, the process further includes: separating the obtained product, and sequentially washing and drying the obtained precipitate to obtain a sodium iron phosphate positive electrode material.

[0059] In some embodiments, the feed rates of the solution comprising the sodium source and the solution comprising the iron source are each independently 1 mL / min to 10 mL / min.

[0060] In some embodiments, the coprecipitation reaction is carried out in a reactor.

[0061] Another embodiment of the present application provides a sodium iron phosphate positive electrode material, which is prepared by the above-mentioned preparation method of the present application. The sodium iron phosphate positive electrode material obtained by the above-mentioned preparation method of the present application has higher purity, better crystallinity, and smaller average particle size, and can improve the electrochemical performance of the sodium ion battery containing the sodium iron phosphate positive electrode material, such as gram capacity, rate performance, low temperature performance and cycle stability.

[0062] In some embodiments, the average particle size of the sodium iron phosphate cathode material is 50 nm to 150 nm. The average particle size of the sodium iron phosphate cathode material is within the above range, which can better exert the electrochemical properties of the sodium iron phosphate cathode material, such as gram capacity, rate performance, low temperature performance and cycle stability.

[0063] In some embodiments, the purity of the sodium iron phosphate positive electrode material is 98% to 99.99%.

[0064] Another embodiment of the present application provides a positive electrode plate, including the sodium iron phosphate positive electrode material mentioned above in the present application.

[0065] The positive electrode sheet comprises a positive electrode current collector and a positive electrode active layer located on at least one side of the positive electrode current collector, wherein the positive electrode active layer comprises a positive electrode active material, a conductive agent and a binder. The positive electrode active material comprises the above-mentioned sodium iron phosphate positive electrode material, and the conductive agent and the binder can adopt the conductive agent and the binder commonly used in the technical field.

[0066] Another embodiment of the present application further provides a sodium ion battery, comprising the sodium iron phosphate positive electrode material mentioned above in the present application and at least one of the positive electrode plates mentioned above in the present application.

[0067] The above-mentioned sodium ion battery may include, for example, the above-mentioned positive electrode sheet, negative electrode sheet, electrolyte and diaphragm. The diaphragm is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, and at the same time to allow active ions to pass through. The electrolyte plays a role in conducting active ions between the positive electrode sheet and the negative electrode sheet. During the charge and discharge process of the sodium ion battery, the active ions are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet.

[0068] Furthermore, another embodiment of the present application further provides an electrical device, including the sodium ion battery of the present application. The electrical device may include any device or apparatus using a secondary battery as a driving source, such as a mobile phone, a laptop computer, an electric vehicle, a ship, a satellite, an energy storage device, etc., but is not limited thereto.

[0069] In order to further illustrate the present application, the technical scheme of the present application is described in detail below in conjunction with specific examples. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in the field or the product instructions are used. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0070] Example 1

[0071] The preparation method of sodium iron phosphate positive electrode material is as follows:

[0072] Step 1: Weigh 10 g of sodium phosphate (phosphorus source) and 7 g of phosphoric acid (pH adjuster) and dissolve them in 400 mL of water (first solvent) to obtain a first mixed solution. Adjust the pH of the mixed solution to 6 and add it to a reactor. Set the temperature to 100° C. and stir at a speed of 300 r / min.

[0073] Step 2: weigh 82 g of sodium phosphate (sodium source) and dissolve it in 1.35 L of deionized water (second solvent) to form solution A (solution containing the sodium source), and dissolve 139 g of ferrous sulfate heptahydrate (iron source) in 250 mL of deionized water (third solvent) to form solution B (solution containing the iron source);

[0074] Step 3: After the temperature of the reactor is raised to 100°C, solution A and solution B are added simultaneously to ensure that both solutions are added at the same time. Feed for 1 hour and adjust the pH value of the obtained second mixed solution to 6 using phosphoric acid or sodium hydroxide;

[0075] Step 4: The second mixed solution is kept at 100° C. and argon atmosphere for 6 hours for co-precipitation reaction, and the pressure of the co-precipitation reaction is 0.1 MPa;

[0076] Step 5: After the reaction is completed, the product is collected, filtered, rinsed and dried to obtain the sodium iron phosphate positive electrode material. After rinsing with an appropriate amount of water and a small amount of ethanol, it is dried in an oven at about 70°C. The XRD (X-ray diffraction pattern) of the test is as follows: Figure 1 shown.

[0077] Example 2

[0078] The preparation method of sodium iron phosphate positive electrode material is as follows:

[0079] Step 1: Weigh 10 g of sodium phosphate (phosphorus source) and 10 g of phosphoric acid (pH adjuster) and dissolve them in 400 mL of water (first solvent) to obtain a first mixed solution. Adjust the pH of the mixed solution to 5 and add it to a reactor. Set the temperature to 100 ° C and stir at a speed of 300 r / min.

[0080] Step 2: weigh 82 g of sodium phosphate (sodium source) and dissolve it in 1.35 L of deionized water (second solvent) to form solution A (solution containing the sodium source), and dissolve 139 g of ferrous sulfate heptahydrate (iron source) in 250 mL of deionized water (third solvent) to form solution B (solution containing the iron source);

[0081] Step 3: After the temperature of the reactor is raised to 100°C, solution A and solution B are added simultaneously to ensure that both solutions are added at the same time. The feed is continued for 1 hour, and the pH value of the obtained second mixed solution is adjusted to 5 using phosphoric acid or sodium hydroxide;

[0082] Step 4: The second mixed solution is kept at 100° C. and argon atmosphere for 6 hours for co-precipitation reaction, and the pressure of the co-precipitation reaction is 0.1 MPa;

[0083] Step 5: After the reaction is completed, the product is collected, filtered, rinsed and dried to obtain a sodium iron phosphate positive electrode material, wherein the product is rinsed with an appropriate amount of water and a small amount of ethanol, and then dried in an oven at about 70°C.

[0084] Example 3

[0085] Step 1: Weigh 10 g of sodium phosphate (phosphorus source) and 3 g of phosphoric acid (pH adjuster) and dissolve them in 400 mL of water (first solvent) to obtain a first mixed solution. Adjust the pH of the mixed solution to 7 and add it to a reactor. Set the temperature to 100° C. and stir at a speed of 300 r / min.

[0086] Step 2: weigh 82 g of sodium phosphate (sodium source) and dissolve it in 1.35 L of deionized water (second solvent) to form solution A (solution containing the sodium source), and dissolve 139 g of ferrous sulfate heptahydrate (iron source) in 250 mL of deionized water (third solvent) to form solution B (solution containing the iron source);

[0087] Step 3: After the temperature of the reactor is raised to 100°C, solution A and solution B are added simultaneously to ensure that both solutions are added at the same time. The feed is continued for 1 hour, and the pH value of the obtained second mixed solution is adjusted to 7 using phosphoric acid or sodium hydroxide;

[0088] Step 4: The second mixed solution is kept at 100° C. and argon atmosphere for 6 hours for co-precipitation reaction, and the pressure of the co-precipitation reaction is 0.1 MPa;

[0089] Step 5: After the reaction is completed, the product is collected, filtered, rinsed and dried to obtain a sodium iron phosphate positive electrode material, wherein the product is rinsed with an appropriate amount of water and a small amount of ethanol, and then dried in an oven at about 70°C.

[0090] Example 4

[0091] Step 1: Weigh 10 g of sodium phosphate (phosphorus source) and 7 g of phosphoric acid (pH adjuster) and dissolve them in 400 mL of water (first solvent) to obtain a first mixed solution. Adjust the pH of the mixed solution to 6 and add it to a reactor. Set the temperature to 110° C. and stir at a speed of 300 r / min.

[0092] Step 2: weigh 82 g of sodium phosphate (sodium source) and dissolve it in 1.35 L of deionized water (second solvent) to form solution A (solution containing the sodium source), and dissolve 87 g of ferrous acetate (iron source) in 250 mL of deionized water (third solvent) to form solution B (solution containing the iron source);

[0093] Step 3: After the temperature of the reactor is raised to 110°C, solution A and solution B are added simultaneously to ensure that both solutions are added at the same time. The mixture is fed for 1 hour and the pH value of the obtained second mixed solution is adjusted to 6 using phosphoric acid or sodium hydroxide.

[0094] Step 4: The second mixed solution is kept at 110° C. and argon atmosphere for 6 hours to perform a coprecipitation reaction, and the pressure of the coprecipitation reaction is 0.2 MPa;

[0095] Step 5: After the reaction is completed, the product is collected, filtered, rinsed and dried to obtain a sodium iron phosphate positive electrode material, wherein the product is rinsed with an appropriate amount of water and a small amount of ethanol, and then dried in an oven at about 70°C.

[0096] Example 5

[0097] The preparation method of the sodium iron phosphate positive electrode material is basically the same as that in Example 1, except that: in step 1, 10 g of sodium phosphate (phosphorus source) and 14 g of phosphoric acid (pH regulator) are weighed and dissolved in 400 mL of water (first solvent) to obtain a first mixed solution, the pH of the mixed solution is adjusted to 4, and the mixed solution is added to a reactor, the temperature is set to 100 ° C, and the stirring speed is 300 r / min; in step 3, phosphoric acid or sodium hydroxide is used to adjust the pH value of the second mixed solution to 4.

[0098] Example 6

[0099] The preparation method of the sodium iron phosphate positive electrode material is basically the same as that in Example 1, except that: in step 1, 10 g of sodium phosphate (phosphorus source) and 1 g of phosphoric acid (pH regulator) are weighed and dissolved in 400 mL of water (first solvent) to obtain a first mixed solution, the pH of the mixed solution is adjusted to 8, and the mixed solution is added to a reactor, the temperature is set to 100 ° C, and the stirring speed is 300 r / min; in step 3, phosphoric acid or sodium hydroxide is used to adjust the pH value of the second mixed solution to 8.

[0100] Comparative Example 1

[0101] The preparation method of the sodium iron phosphate positive electrode material is basically the same as that in Example 1, except that: in step 1, 10 g of sodium phosphate (phosphorus source) and 0.5 g of phosphoric acid (pH regulator) are weighed and dissolved in 400 mL of water (first solvent) to obtain a first mixed solution, the pH of the mixed solution is adjusted to 10, and the mixed solution is added to a reactor, the temperature is set to 100 ° C, and the stirring speed is 300 r / min; in step 3, the pH value of the second mixed solution is adjusted to 10 using phosphoric acid or sodium hydroxide.

[0102] Comparative Example 2

[0103] The preparation method of sodium iron phosphate positive electrode material is as follows:

[0104] Weigh 2.23 g of ferrous gluconate, 8.99 g of ferrous oxalate, 2.65 g of sodium carbonate, and 5.75 g of ammonium dihydrogen phosphate, mix and dissolve the above materials in 25 mL of deionized water, and then transfer them to a ball mill for wet ball milling at a speed of 500 rpm / min and a ball milling time of 4 h. After the wet ball milling is completed, the slurry in the ball mill is collected and placed in a vacuum drying oven for drying. After drying, the material is collected and then placed in a ball mill for ball milling at a speed of 300 rpm / min and a ball milling time of 1 h to obtain a precursor powder.

[0105] The precursor powder is placed in a tubular furnace for sintering, the air in the furnace tube is evacuated with high-purity nitrogen, and then sintering is carried out in a high-purity nitrogen atmosphere. The sintering system is: first, the temperature is increased to 300°C at a rate of 5°C / min, pre-sintering for 4 hours, and then the temperature is continued to be increased to 600°C at a rate of 5°C / min and sintered for 10 hours to obtain a sodium iron phosphate positive electrode material.

[0106] Test Case

[0107] (1) Crystallinity test of sodium iron phosphate positive electrode material:

[0108] The crystallinity of the sodium iron phosphate positive electrode material was tested using XRD test.

[0109] Figure 1 The XRD pattern of the sodium iron phosphate positive electrode material prepared in Example 1 is shown. Figure 1 In the figure, the black curve indicates the peak position of sodium iron phosphate in the PDF card. Figure 1 It can be seen that Example 1 successfully prepared the sodium iron phosphate positive electrode material, and each diffraction peak was relatively sharp, indicating that the sodium iron phosphate positive electrode material prepared in Example 1 had good crystallinity.

[0110] (2) Average particle size test of sodium iron phosphate positive electrode material:

[0111] The average particle size of the sodium iron phosphate positive electrode material was tested using a particle size analyzer.

[0112] (3) Purity test of sodium iron phosphate positive electrode material:

[0113] By performing XRD diffraction on a 100% pure sample, the characteristic peak intensity is selected as the benchmark I0. In the XRD diffraction pattern of the sample test, the ratio of the characteristic peak intensity I to I0 is defined as the purity.

[0114] (4) Preparation of batteries:

[0115] The sodium iron phosphate positive electrode material prepared in each embodiment or each comparative example is used as the positive electrode active material, SP is selected as the conductive agent, PVDF is selected as the binder, and NMP is selected as the solvent. The positive electrode active material, the conductive agent and the binder are evenly mixed in a mass ratio of 8:1:1 to form a slurry, which is then coated on an aluminum foil, dried and cut into positive electrode discs, a sodium sheet is used as a counter electrode, a polypropylene diaphragm is used as a diaphragm, and button cells are assembled in a glove box. The electrolyte is 1M NaPF6 dissolved in a mixed solution of ethylene carbonate (EC), diethyl carbonate (DEC) and dimethyl carbonate (DMC) (volume ratio of 1:1:1). After the button cells are assembled, they are left to stand for 12 hours for electrochemical performance testing.

[0116] (5) Battery capacity test:

[0117] The button cell was subjected to the first constant current discharge test and the first constant current charge test at 0.33C rate at 25°C, with a voltage range of 1.5V~4V.

[0118] (6) Battery rate performance test:

[0119] The button battery was charged at a rate of 0.33C at 25°C, and then discharged at a rate of 3C, with a voltage range of 1.5V~4V. Under this temperature condition, the 3C capacity retention rate (%) = capacity corresponding to the 3C rate / capacity corresponding to the 0.33C rate × 100%, which is the rate performance of the battery.

[0120] (7) Low temperature performance test of battery:

[0121] The button cell was charged at a rate of 0.1C and discharged at a rate of 0.33C at -20°C, with a voltage range of 1.5V~4V. Under this temperature condition, the -20°C capacity retention rate (%) = capacity corresponding to the rate of 0.33C / capacity corresponding to the rate of 0.1C × 100%, which is the low temperature performance of the battery.

[0122] (8) Battery cycle performance test:

[0123] The button cell was charged at 1C rate at 25°C, and then discharged at 1C rate. The discharge capacity in the first week was recorded as C0. The cycle was repeated for 50 weeks, and the discharge capacity in the 50th week was recorded as C1. The voltage range was 1.5V~4V.

[0124] The capacity retention rate (%) at the 50th week = C1 / C0×100%. The higher the capacity retention rate, the better the battery's cycle performance.

[0125] The test results of each embodiment and each comparative example are shown in Table 1.

[0126] Table 1

[0127]

[0128] From the data in Table 1, we can see the following:

[0129] The pH value of the mixed solution in Comparative Example 1 is 10. Comparative Example 2 uses a traditional solid phase method to prepare a sodium iron phosphate positive electrode material. Compared with the sodium iron phosphate positive electrode material prepared in Comparative Examples 1 to 2, the purity of the sodium iron phosphate positive electrode material prepared in Examples 1 to 6, as well as the first discharge gram capacity, 3C capacity retention rate, -20°C capacity retention rate, and 50-week capacity retention rate of the assembled battery are higher, indicating that the preparation method used in Examples 1 to 6 can improve the purity of the prepared sodium iron phosphate positive electrode material, and can improve the gram capacity, rate performance, low temperature performance, and cycle performance of the battery containing the sodium iron phosphate positive electrode material. In addition, the preparation method of Examples 1 to 6 also has the advantages of simple process, energy saving, environmental protection, and high safety performance.

[0130] The present application also tests the yield of the sodium iron phosphate positive electrode material prepared by the preparation methods of Example 1 and Comparative Examples 1-2, and the test results are 99%, 78% and 94%, respectively. This shows that the preparation method provided by the present application can also significantly improve the yield of the sodium iron phosphate positive electrode material.

[0131] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0132] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims, and the description may be used to interpret the content of the claims.

Claims

1. A method for preparing a sodium iron phosphate positive electrode material, characterized in that: The steps include: Mixing the phosphorus source and the first solvent, and adjusting the pH value of the obtained first mixed solution to 4-8; Adding a solution containing a sodium source and a solution containing an iron source to the first mixed solution at the same time, and adjusting the pH value of the obtained second mixed solution to be the same as the pH value of the first mixed solution; The second mixed solution is subjected to a coprecipitation reaction under protective atmosphere conditions, and the process conditions of the coprecipitation reaction include: a reaction temperature of 95° C. to 160° C. and a reaction time of 4 h to 10 h to prepare the sodium iron phosphate positive electrode material.

2. The preparation method according to claim 1, characterized in that: The process conditions of the coprecipitation reaction also include: a pressure of 0.1 MPa to 0.4 MPa.

3. The preparation method according to claim 1, characterized in that: The preparation method meets at least one of the following conditions (1) to (3): (1) before the step of simultaneously adding the solution containing the sodium source and the solution containing the iron source to the first mixed solution, the method further comprises: heating the first mixed solution to a temperature of 95° C. to 160° C.; (2) the step of mixing the phosphorus source and the first solvent, and adjusting the pH value of the obtained first mixed solution to 4-8 comprises: using a first pH adjuster to adjust the pH value of the first mixed solution to 4-8; (3) The step of simultaneously adding a solution containing a sodium source and a solution containing an iron source to the first mixed solution, and adjusting the pH value of the resulting second mixed solution to be the same as the pH value of the first mixed solution comprises: using a second pH adjuster to adjust the pH value of the second mixed solution to 4-8.

4. The preparation method according to claim 3, characterized in that: The first pH adjuster and the second pH adjuster each independently include one or more of phosphoric acid, acetic acid, citric acid, sulfuric acid and sodium hydroxide.

5. The preparation method according to any one of claims 1 to 4, characterized in that The preparation method meets at least one of the following conditions (1) to (7): (1) The concentration of the first mixed solution is 0.1 mol / L to 1 mol / L; (2) The concentration of the solution containing the sodium source is 0.1 mol / L to 1 mol / L; (3) The concentration of the solution containing the iron source is 0.1 mol / L to 1 mol / L; (4) The phosphorus source includes one or more of sodium dihydrogen phosphate, ammonium dihydrogen phosphate, sodium phosphate, potassium dihydrogen phosphate and phosphoric acid; (5) The sodium source includes one or more of sodium dihydrogen phosphate, sodium sulfate, sodium phosphate, sodium acetate and sodium chloride; (6) The iron source includes one or more of ferrous sulfate, ferrous chloride and ferrous acetate; (7) The solution containing the sodium source contains a second solvent, and the solution containing the iron source contains a third solvent, and the first solvent, the second solvent, and the third solvent each independently include one or more of water and alcohol solvents.

6. The preparation method according to any one of claims 1 to 4, characterized in that After the step of subjecting the second mixed solution to a coprecipitation reaction under protective atmosphere conditions, the method further includes: separating the obtained product, and sequentially washing and drying the obtained precipitate to obtain the sodium iron phosphate positive electrode material.

7. A sodium iron phosphate positive electrode material, characterized in that: The method is prepared according to any one of claims 1 to 6.

8. The sodium iron phosphate positive electrode material according to claim 7, characterized in that The sodium iron phosphate positive electrode material has at least one of the following characteristics (1) to (2): (1) The average particle size of the sodium iron phosphate positive electrode material is 50nm~150nm; (2) The purity of the sodium iron phosphate positive electrode material is 98% to 99.99%.

9. A positive electrode sheet, characterized in that: The invention comprises the sodium iron phosphate positive electrode material according to any one of claims 7 to 8.

10. A sodium ion battery, characterized in that: It comprises at least one of the sodium iron phosphate positive electrode material according to any one of claims 7 to 8 and the positive electrode sheet according to claim 9.

Citation Information

Patent Citations

  • Hydrothermal synthesis method of LiFePO4 of anode material of lithium ion battery with one-dimensional nanometer structure

    CN101752564A

  • Preparation method of sodium-ion battery cathode material as well as product and application of sodium-ion battery cathode material

    CN105789617A

  • Sodium ferric phosphate material and preparation method thereof

    CN116750742A

  • Electrode material and method of synthesizing

    US20150132640A1

Cited By

  • Sodium-ion battery positive electrode, preparation method thereof and sodium-ion battery

    CN122370334A