Preparation method of low-ash columnar coal-based activated carbon
By mixing and modifying Taixi coal powder, the pore structure of activated carbon is optimized, and the problems of difficult activation and high fever loss in Taixi coal are solved when preparing activated carbon, and efficient activated carbon production is achieved, and low ash content and excellent production is prepared. Activated carbon products with pore structure.
Patent Information
- Application Number
- CN202411276565.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-12
AI Technical Summary
When using Taixi coal to prepare columnar activated carbon, its characteristics lead to difficulty in activation, high firing loss rate, large production cost and energy consumption, and low output.
By mixing and modifying raw materials to Taixi coal powder, the pore structure of activated carbon is optimized, the contact area of activator is increased, and the firing loss rate and energy consumption are reduced. The ball milling mechanism powder, kneading and molding technology is used, and the micro powder ultra-pure carbon and coal are combined with micro powder. Excipients such as tar, lignin and caprolactone form a messy pore structure to improve activation efficiency.
It effectively reduces the firing loss rate and energy consumption of activated carbon, improves the activation yield and yield, solves the problems of difficulty in activation and low yield, and the prepared activated carbon has high strength, low ash content and excellent pore structure.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of activated carbon preparation, and in particular to a method for preparing low-ash columnar coal-based activated carbon. Background Art
[0002] As my country's requirements for environmental protection continue to increase, more and more types of air pollutants are being controlled, emission standards are becoming increasingly stringent, and the demand for pollutant control in industrial flue gas is becoming more urgent. Activated carbon flue gas purification technology has many significant advantages, such as the combined removal of multiple pollutants, high efficiency of desulfurization and denitrification, and recoverable sulfur resources. It can provide a comprehensive solution for solving air pollution control. As an effective material for purifying flue gas and impurity particles, activated carbon has been widely studied and applied at home and abroad. Traditional activated carbon mainly uses raw coal, coal tar and asphalt as raw materials. The production process mainly includes coal blending, grinding, kneading, molding, drying, carbonization, activation, screening and packaging. At present, most domestic activated carbon manufacturers use coking coal, bituminous coal, semi-coke or anthracite of good quality as raw materials.
[0003] Taixi coal is a high-quality coal with the characteristics of three lows (low phosphorus, low ash, and low sulfur) and six highs (high calorific value, high lump coal rate, high specific resistivity, high chemical activity, high clean coal recovery rate, and high mechanical strength). Therefore, it is one of the preferred raw materials for low-ash activated carbon. However, when using Taixi coal as a raw material to prepare columnar activated carbon, due to the limitations of the characteristics of Taixi coal itself and the small specific surface area of columnar activated carbon, it has application defects such as difficulty in activation, high ignition loss rate, and high production ton consumption. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for preparing low-ash columnar coal-based activated carbon. By blending and modifying Taixi coal powder as raw materials, the pore structure of the activated carbon is optimized, the activated carbon is facilitated to contact and activate with an activator, the loss on ignition rate as well as resource consumption and energy consumption are reduced, and the problems of difficulty in activation, low yield and high energy consumption associated with the use of high-quality coal in the activated carbon industry to produce columnar activated carbon are solved.
[0005] The present invention provides a method for preparing low-ash columnar coal-based activated carbon, comprising the following steps:
[0006] (1) Powdering: The raw materials, Taixi coal and ultra-pure carbon, are crushed by a crusher, then ground by a ball mill and sieved, and the Taixi coal powder and ultra-pure carbon powder with a size less than 200 mesh are taken for use;
[0007] (2) Ingredients: Weigh 50-70 parts of Taixi coal, 30-50 parts of ultra-pure carbon powder, 33-34 parts of coal tar, 3-10 parts of lignin, 1-3 parts of caprolactone, 1-3 parts of oxalic acid and 0.5-1 part of triethylamine according to weight; preliminarily mix the Taixi coal and the ultra-pure carbon powder to obtain a mixed powder A; dissolve the lignin in a suitable amount of dimethylacetamide at a temperature of 40-60° C., then add coal tar and mix for 5-10 minutes to obtain a mixed solution B; add oxalic acid and triethylamine to a suitable amount of dimethylacetamide at a temperature of 40-60° C., and mix well to obtain a mixed solution C;
[0008] (3) Kneading and molding: Add the mixed powder A to a kneader at a constant temperature of 60 to 100° C. and mix evenly, then add the mixed solution B to it and mix for 5 to 10 minutes, then add the mixed solution C to it and stir and knead for 10 to 20 minutes to obtain coal slime; the obtained coal slime is extruded into coal strips with a diameter of 1.8 mm on a molding device, and spread flat to dry naturally;
[0009] (4) Carbonization: The carbonization furnace is heated to 280-320° C., the sample tube containing the coal strips obtained in step (3) is placed in the carbonization furnace, the temperature is increased to 550-650° C. at a heating rate of 10° C. / min, and the temperature is kept at that temperature for 40-60 min to complete carbonization, and the carbonized material is obtained by cooling, discharging and weighing;
[0010] (5) Activation: The activation furnace is heated to 550-650° C., the sample tube containing the carbonized material obtained in step (4) is placed in the activation furnace, and the temperature is raised to 850-950° C. at a heating rate of 10° C. / min, and dimethylacetamide vapor is passed at a flow rate of 10 mL / min, and the activation is completed by keeping the temperature for 60-100 min;
[0011] (6) Discharging: Cut off the power supply, turn off the dimethylacetamide vapor, cool naturally, and screen to remove broken materials and dust after discharging to obtain activated carbon products.
[0012] Preferably, the mixed solution B in step (2) further comprises 1 to 3 parts of caprolactone.
[0013] Preferably, the step (2) comprises 60 parts of Taixi coal, 40 parts of ultrapure carbon powder, 33 parts of coal tar, 5 parts of lignin, 2 parts of caprolactone, 2 parts of oxalic acid and 0.7 parts of triethylamine.
[0014] Preferably, the total amount of dimethylacetamide used in the mixed solution B and the mixed solution C in step (2) is 12 to 15 parts.
[0015] Preferably, the ultrapure carbon powder has an ash content of 2-3Ad%, a volatile matter of <8Vd%, a sulfur content of 0.7-1St,d%, a particle size of 15 (D90) μm, a calorific value of >8000Qnet.aR kcal / kg, a fixed carbon content of ≥90FCd%, a water content of <25Mt%, and a tap density of 0.4-0.5t / m 3 Specific surface area: 55m 2 / g;
[0016] The Taixi coal has an ash content of ≤12Ad%, a volatile matter of <10Vd%, a sulfur of <1.3St,d%, a calorific value of >7000Qnet.aR kcal / kg, and a water content of <18Mt%.
[0017] Preferably, the temperature of the dimethylacetamide in step (2) is 50°C, and the temperature of the kneader in step (3) is 90°C.
[0018] Preferably, the coal tar in step (2) has an asphalt content greater than 65.9, a light oil content ≤2.46%, a heavy oil content ≤21.22, a dimethylacetamide content ≤0.28%, and an ash content ≤0.06.
[0019] Preferably, the carbonization process in step (4) is as follows: heating the carbonization furnace to 300°C, placing the sample tube containing the coal strips obtained in step (3) into the carbonization furnace, heating the temperature to 600°C at a heating rate of 10°C / min, and then keeping the temperature for 45 minutes to complete the carbonization, cooling to obtain the carbonized material, discharging the material and weighing it.
[0020] Preferably, the activation process in step (5) is as follows: the activation furnace is heated to 600°C, the sample tube containing the carbonized material obtained in step (4) is placed in the activation furnace, the temperature is raised to 920°C at a heating rate of 10°C / min, dimethylacetamide vapor is passed at a flow rate of 10 mL / min, and the activation is completed by keeping the temperature for 90 minutes.
[0021] Working principle of the present invention:
[0022] First of all, the micro-powder ultra-pure carbon has the characteristics of low ash, low sulfur, and high fixed carbon content. It is mixed with Taixi coal as the main raw material, and the auxiliary materials are all organic materials. No activated carbon ash is produced at high temperature, and the prepared activated carbon has the characteristics of low ash.
[0023] Secondly, micro-powder ultra-pure carbon contains more cellulose carbon and silk carbon, which is easy to form more randomly arranged pore structures when heated, and is easy to activate and form pores. The present invention uses Taixi coal doped with micro-powder ultra-pure carbon to prepare activated carbon, changes the pore structure of activated carbon products produced by a single type of coal, reduces the number of micropores, increases the number of medium and large pores, forms a randomly arranged pore structure, and optimizes the pore structure of activated carbon. By optimizing the pore structure, water vapor can evenly and quickly react with the inside and surface of carbon particles to activate, reduce carbon burning loss, improve activation yield and efficiency as well as single furnace output, reduce energy consumption in activated carbon production, and ultimately solve the problem of difficult activation and high ton consumption of Taixi coal.
[0024] In addition, there are active groups such as aromatic groups, phenolic hydroxyl groups, alcoholic hydroxyl groups, carbonyl conjugated double bonds in the molecular structure of lignin, so chemical reactions such as polycondensation or graft copolymerization can be carried out. In the present invention, in step (3), mixed powder A is added to a kneader for uniform mixing, and then mixed solution B is added thereto, aromatic hydrocarbons and heterocyclic organic compounds in coal tar are used to react with lignin to increase active groups, and then mixed solution C is added thereto for stirring and kneading, and oxalic acid and lignin undergo polycondensation under the catalytic action of triethylamine to form a network structure and coat the mixed powder. In addition, the caprolactone molecule contains a five-membered lactone ring and an alkyl side chain, and the presence of the alkyl side chain makes caprolactone have good solubility and compatibility in the solvent. Since the caprolactone molecule contains a carbonyl group, it has a certain reactivity, and various chemical reactions such as esterification, addition, and nucleophilic substitution can occur, which is convenient for polycondensation with lignin to form a more complete network structure. The lignin network structure and the asphalt in coal tar work together to improve the cohesiveness of the powder, and form a polymer protective film on the surface of the activated carbon after molding, which can reduce the burning loss rate of activated carbon and prevent the activated carbon from breaking during processing. At the same time, the condensation products and the oily components of light oil and heavy oil in coal tar decompose during the carbonization process, further enriching and optimizing the pore structure of activated carbon.
[0025] Beneficial effects of the present invention: The preparation method of low-ash columnar coal-based activated carbon of the present invention analyzes and screens the feasibility of coal blending from the perspective of coal quality analysis and coal reaction activity, and uses Taixi coal doped with micro-powdered ultra-pure carbon to prepare activated carbon. The technology of preparing activated carbon by doping with coal blending changes the pore structure of activated carbon products produced by a single type of coal, effectively changes the pore distribution of Taixi coal-based activated carbon, reduces the number of micropores, increases the number of medium and large pores, and forms a randomly arranged pore structure. By forming larger and randomly arranged pores, water vapor can evenly and quickly react with the inside and surface of carbon particles to activate, reduce carbon burnout, and improve activation yield, efficiency and single furnace output. After the raw materials are subjected to key processes such as kneading, molding, carbonization, and activation, the yield of activated carbon is not less than 45%. In addition, lignin is used to undergo a polycondensation reaction as a binder and protective film to improve the quality of activated carbon. The present invention solves the problems of difficult activation, small pore structure, and poor decolorization effect in the preparation of activated carbon from Taixi coal. The technical indicators of the product prepared by the invention are as follows: ash content ≤8%, strength ≥96%, bulk density 480±g / L, iodine value ≥1000mg / g, CTC ≥60%, dimethylacetamide capacity ≥80%, and methylene blue ≥220mg / g. DETAILED DESCRIPTION
[0026] In order to make the technical solution of the present invention easier to understand, the technical solution of the present invention is now clearly and completely described in the form of specific embodiments.
[0027] Embodiment 1:
[0028] The method for preparing low-ash columnar coal-based activated carbon of this embodiment comprises the following steps:
[0029] (1) Powdering: The raw materials, Taixi coal and ultra-pure carbon, are crushed by a crusher, then ground by a ball mill and sieved, and the Taixi coal powder and ultra-pure carbon powder with a size less than 200 mesh are taken for use;
[0030] (2) Ingredients: Weigh 50 parts of Taixi coal, 50 parts of ultra-pure carbon powder, 33 parts of coal tar, 10 parts of lignin, 1 part of oxalic acid and 1 part of triethylamine according to weight; preliminarily mix the Taixi coal and ultra-pure carbon powder to obtain a mixed powder A; dissolve the lignin in a suitable amount of dimethylacetamide at a temperature of 40° C., then add coal tar and mix for 10 minutes to obtain a mixed solution B; add oxalic acid and triethylamine to a suitable amount of dimethylacetamide at a temperature of 40° C., and mix well to obtain a mixed solution C;
[0031] (3) Kneading and molding: Mixed powder A is added to a kneading machine at a constant temperature of 60°C and mixed evenly, and then mixed liquid B is added thereto and mixed for 10 minutes, and then mixed liquid C is added thereto and stirred and kneaded for 100 minutes to obtain coal slime; the obtained coal slime is extruded into coal strips with a diameter of 1.8 mm on a molding device, and then spread flat and dried naturally;
[0032] (4) Carbonization: The carbonization furnace is heated to 280° C., the sample tube containing the coal strips obtained in step (3) is placed in the carbonization furnace, the temperature is increased to 550° C. at a heating rate of 10° C. / min, and the temperature is kept for 60 min to complete carbonization, and the carbonized material is obtained by cooling, discharging and weighing;
[0033] (5) Activation: The activation furnace is heated to 550° C., the sample tube containing the carbonized material obtained in step (4) is placed in the activation furnace, the temperature is raised to 850° C. at a heating rate of 10° C. / min, dimethylacetamide vapor is passed at a flow rate of 10 mL / min, and the activation is completed by keeping the temperature for 100 min;
[0034] (6) Discharging: Cut off the power supply, turn off the dimethylacetamide vapor, cool naturally, and screen to remove broken materials and dust after discharging to obtain activated carbon products.
[0035] Embodiment 2:
[0036] The method for preparing low-ash columnar coal-based activated carbon of this embodiment comprises the following steps:
[0037] (1) Powdering: The raw materials, Taixi coal and ultra-pure carbon, are crushed by a crusher, then ground by a ball mill and sieved, and the Taixi coal powder and ultra-pure carbon powder with a size less than 200 mesh are taken for use;
[0038] (2) Ingredients: Weigh 60 parts of Taixi coal, 40 parts of ultra-pure carbon powder, 33 parts of coal tar, 5 parts of lignin, 2 parts of caprolactone, 2 parts of oxalic acid and 0.7 parts of triethylamine according to weight; preliminarily mix the Taixi coal and the ultra-pure carbon powder to obtain a mixed powder A; dissolve lignin and caprolactone in a suitable amount of dimethylacetamide at a temperature of 50° C., then add coal tar and mix for 8 minutes to obtain a mixed solution B; add oxalic acid and triethylamine to a suitable amount of dimethylacetamide at a temperature of 50° C., and mix well to obtain a mixed solution C;
[0039] (3) Kneading and molding: Mixed powder A is added to a kneading machine at a constant temperature of 90°C and mixed evenly, and then mixed liquid B is added thereto and mixed for 8 minutes, and then mixed liquid C is added thereto and stirred and kneaded for 15 minutes to obtain coal slime; the obtained coal slime is extruded into coal strips with a diameter of 1.8 mm on a molding device, and spread flat to dry naturally;
[0040] (4) Carbonization: Heat the carbonization furnace to 300° C., place the sample tube containing the coal strips obtained in step (3) into the carbonization furnace, heat the furnace to 600° C. at a heating rate of 10° C. / min, and then keep the temperature for 45 min to complete carbonization. Cool the carbonized material to obtain the carbonized material, discharge the material and weigh it;
[0041] (5) Activation: The activation furnace is heated to 600° C., the sample tube containing the carbonized material obtained in step (4) is placed in the activation furnace, the temperature is raised to 920° C. at a heating rate of 10° C. / min, dimethylacetamide vapor is passed at a flow rate of 10 mL / min, and the activation is completed by keeping the temperature for 90 min;
[0042] (6) Discharging: Cut off the power supply, turn off the dimethylacetamide vapor, cool naturally, and screen to remove broken materials and dust after discharging to obtain activated carbon products.
[0043] Embodiment 3:
[0044] The method for preparing low-ash columnar coal-based activated carbon of this embodiment comprises the following steps:
[0045] (1) Powdering: The raw materials, Taixi coal and ultra-pure carbon, are crushed by a crusher, then ground by a ball mill and sieved, and the Taixi coal powder and ultra-pure carbon powder with a size less than 200 mesh are taken for use;
[0046] (2) Ingredients: 70 parts of Taixi coal, 30 parts of ultra-pure carbon powder, 34 parts of coal tar, 3 parts of lignin, 3 parts of caprolactone, 3 parts of oxalic acid and 0.5 parts of triethylamine were weighed according to weight; Taixi coal and ultra-pure carbon powder were preliminarily mixed to obtain mixed powder A; lignin and caprolactone were dissolved in a suitable amount of dimethylacetamide at a temperature of 60° C., and then coal tar was added and mixed for 5 minutes to obtain a mixed solution B; oxalic acid and triethylamine were added to a suitable amount of dimethylacetamide at a temperature of 60° C., and mixed uniformly to obtain a mixed solution C;
[0047] (3) Kneading and molding: Mixed powder A is added to a kneading machine at a constant temperature of 100°C and mixed evenly, and then mixed liquid B is added thereto and mixed for 5 minutes, and then mixed liquid C is added thereto and stirred and kneaded for 20 minutes to obtain coal slime; the obtained coal slime is extruded into coal strips with a diameter of 1.8 mm on a molding device, and spread flat to dry naturally;
[0048] (4) Carbonization: The carbonization furnace is heated to 320° C., the sample tube containing the coal strips obtained in step (3) is placed in the carbonization furnace, the temperature is increased to 650° C. at a heating rate of 10° C. / min, and the temperature is kept at this temperature for 40 min to complete the carbonization, the carbonized material is cooled, the material is discharged and weighed;
[0049] (5) Activation: The activation furnace is heated to 650° C., the sample tube containing the carbonized material obtained in step (4) is placed in the activation furnace, the temperature is raised to 950° C. at a heating rate of 10° C. / min, dimethylacetamide vapor is passed at a flow rate of 10 mL / min, and the activation is completed by keeping the temperature for 60 min;
[0050] (6) Discharging: Cut off the power supply, turn off the dimethylacetamide vapor, cool naturally, and screen to remove broken materials and dust after discharging to obtain activated carbon products.
[0051] It should be noted that the embodiments described herein are only partial embodiments of the present invention, rather than all implementations of the present invention, and the embodiments are only exemplary, and their role is only to provide a more intuitive and clear way to understand the content of the present invention, rather than to limit the technical solutions described in the present invention. Without departing from the concept of the present invention, all other implementation methods that can be thought of by ordinary technicians in this field without creative work, and other simple replacements and various changes to the technical solutions of the present invention, all belong to the protection scope of the present invention.
Claims
1. A method for preparing low-ash columnar coal-based activated carbon, It is characterized in that The following steps are involved: (1) Powdering: The raw materials, Taixi coal and ultra-pure carbon, are crushed by a crusher, then ground by a ball mill and sieved, and the Taixi coal powder and ultra-pure carbon powder with a size less than 200 mesh are taken for use; (2) Ingredients: Weigh 50-70 parts of Taixi coal, 30-50 parts of ultra-pure carbon powder, 33-34 parts of coal tar, 3-10 parts of lignin, 1-3 parts of oxalic acid and 0.5-1 part of triethylamine according to weight; preliminarily mix the Taixi coal and the ultra-pure carbon powder to obtain a mixed powder A; dissolve the lignin in a suitable amount of dimethylacetamide at a temperature of 40-60° C., then add the coal tar and mix for 5-10 minutes to obtain a mixed solution B; add oxalic acid and triethylamine to a suitable amount of dimethylacetamide at a temperature of 40-60° C., and mix them evenly to obtain a mixed solution C; (3) Kneading and molding: Add the mixed powder A to a kneader at a constant temperature of 60 to 100° C. and mix evenly, then add the mixed solution B to it and mix for 5 to 10 minutes, then add the mixed solution C to it and stir and knead for 10 to 20 minutes to obtain coal slime; the obtained coal slime is extruded into coal strips with a diameter of 1.8 mm on a molding device, and spread flat to dry naturally; (4) Carbonization: The carbonization furnace is heated to 280-320° C., the sample tube containing the coal strips obtained in step (3) is placed in the carbonization furnace, the temperature is increased to 550-650° C. at a heating rate of 10° C. / min, and the temperature is kept at that temperature for 40-60 min to complete carbonization, and the carbonized material is obtained by cooling, discharging and weighing; (5) Activation: The activation furnace is heated to 550-650° C., the sample tube containing the carbonized material obtained in step (4) is placed in the activation furnace, and the temperature is raised to 850-950° C. at a heating rate of 10° C. / min, and dimethylacetamide vapor is passed at a flow rate of 10 mL / min, and the activation is completed by keeping the temperature for 60-100 min; (6) Discharging: Cut off the power supply, turn off the dimethylacetamide vapor, cool naturally, and screen to remove broken materials and dust after discharging to obtain activated carbon products.
2. The method for preparing low-ash columnar coal-based activated carbon according to claim 1, It is characterized in that The mixed solution B in step (2) also includes 1 to 3 parts of caprolactone.
3. The method for preparing low-ash columnar coal-based activated carbon according to claim 2, It is characterized in that In step (2), 60 parts of Taixi coal, 40 parts of ultrapure carbon powder, 33 parts of coal tar, 5 parts of lignin, 2 parts of caprolactone, 2 parts of oxalic acid and 0.7 parts of triethylamine are prepared.
4. The method for preparing low-ash columnar coal-based activated carbon according to claim 1, It is characterized in that The total amount of dimethylacetamide used in the mixed solution B and the mixed solution C in step (2) is 12 to 15 parts.
5. The method for preparing low-ash columnar coal-based activated carbon according to claim 1, It is characterized in that The ultra-pure carbon powder has an ash content of 2-3Ad%, a volatile content of <8Vd%, a sulfur content of 0.7-1St,d%, a particle size of 15 (D90) μm, a calorific value of >8000Qnet.aR kcal / kg, a fixed carbon content of ≥90FCd%, a water content of <25Mt%, and a tap density of 0.4-0.5t / m 3 Specific surface area: 55m 2 / g; The Taixi coal has an ash content of ≤12Ad%, a volatile matter of <10Vd%, a sulfur of <1.3St,d%, a calorific value of >7000Qnet.aRkcal / kg, and a water content of <18Mt%.
6. The method for preparing low-ash columnar coal-based activated carbon according to claim 1, It is characterized in that The temperature of the dimethylacetamide in step (2) is 50°C, and the temperature of the kneader in step (3) is 90°C.
7. The method for preparing low-ash columnar coal-based activated carbon according to claim 1, It is characterized in that The coal tar in step (2) has an asphalt content greater than 65.9, a light oil content less than or equal to 2.46%, a heavy oil content less than or equal to 21.22, a dimethylacetamide content less than or equal to 0.28%, and an ash content less than or equal to 0.
06.
8. The method for preparing low-ash columnar coal-based activated carbon according to claim 1, It is characterized in that The carbonization process described in step (4) is specifically as follows: heating the carbonization furnace to 300°C, placing the sample tube containing the coal strips obtained in step (3) into the carbonization furnace, heating the temperature to 600°C at a heating rate of 10°C / min, and then keeping the temperature for 45 minutes to complete the carbonization, cooling to obtain the carbonized material, discharging the material and weighing it.
9. The method for preparing low-ash columnar coal-based activated carbon according to claim 1, It is characterized in that The specific process of activation in step (5) is as follows: the activation furnace is heated to 600°C, the sample tube containing the carbonized material obtained in step (4) is placed in the activation furnace, the temperature is raised to 920°C at a heating rate of 10°C / min, dimethylacetamide vapor is passed at a flow rate of 10mL / min, and the activation is completed by keeping the temperature for 90min.
Citation Information
Patent Citations
Treatment of carbonaceous feedstocks
CA2914971A1
Columnar activated carbon based on coal pitch binders and preparation method of columnar activated carbon
CN102674341A
Preparation method of columnar bamboo activated carbon
CN104211061A
Tung oil modified bituminous waterproof sheet material
CN105038274A
Additive for improving activated carbon microporous structure and method for preparing activated carbon by using additive
CN112299409A