Preparation method of vanadium dioxide powder
By decomposing ammonium metavanadate into hydrogen under an inert atmosphere, the problems of complex processes and wastewater pollution in the prior art are solved, and the efficient and low-cost preparation of vanadium dioxide powder is achieved, which is suitable for large-scale Large-scale industrial production.
Patent Information
- Application Number
- CN202411224005.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
AI Technical Summary
The existing vanadium dioxide powder preparation method has complex processes, high raw material costs, and the water-based preparation system has wastewater pollution problems.
By mixing high-purity ammonium metavanadate with vanadium pentoxide at high temperature under an inert atmosphere, the hydrogen generated by ammonium metavanadate is reduced and converted into vanadium dioxide is converted to vanadium dioxide, simplifying the process flow, reducing costs, and avoiding the generation of polluted gases. .
It realizes efficient preparation of vanadium dioxide powder, with simple process, environmentally friendly and low cost, and is suitable for large-scale industrial production.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of vanadium dioxide, and particularly relates to a method for preparing vanadium dioxide powder. Background Art
[0002] Vanadium dioxide is a thermotropic phase-change material that undergoes a reversible, heat-induced semiconductor-to-metal phase transition around 70°C. This transition involves a rapid transition from a monoclinic rutile structure (a semiconductor phase) at low temperatures to a tetragonal rutile structure (a metallic phase) at high temperatures. This structural difference before and after the phase transition leads to a sudden change in its electrical, optical, and magnetic properties, making it a promising material for a wide range of applications, including photoelectric conversion, optical storage, energy-saving windows, thermal switches, laser protection, infrared imaging simulation, and transistor circuits.
[0003] Currently, methods for preparing vanadium dioxide powder include hydrothermal synthesis, thermal decomposition, chemical precipitation, and gel-sol methods. However, these methods all suffer from complex preparation processes and high raw material costs. Furthermore, some aqueous preparation systems generate large amounts of wastewater. The present invention is proposed to address at least one of these issues. Summary of the Invention
[0004] The present applicants have discovered that by thoroughly mixing equal amounts of high-purity ammonium metavanadate and high-purity vanadium pentoxide, the high-purity vanadium pentoxide in the system can be completely reduced to high-purity vanadium dioxide using the hydrogen generated by the pyrolysis of the high-purity ammonium metavanadate under an inert atmosphere. This method eliminates the need to reduce the vanadium pentoxide by adding a reducing gas or reducing substance, reducing production costs and generating no polluting gases. The process is simple, environmentally friendly, safe, and operationally sound, making it suitable for large-scale industrial production.
[0005] The specific method of this application is as follows: A method for preparing vanadium dioxide powder, comprising the following steps:
[0006] The same molar number of ammonium metavanadate and vanadium pentoxide are mixed and ball-milled, and calcined at a temperature of 550-650° C. for 2-4 hours under an inert atmosphere to obtain vanadium dioxide powder.
[0007] Preferably, the inert atmosphere is nitrogen, helium, neon, argon, krypton or xenon.
[0008] Preferably, the method specifically includes the following steps:
[0009] Step A: adding equal moles of ammonium metavanadate and vanadium pentoxide into a container and stirring to mix them evenly;
[0010] Step B: placing the mixed material obtained in step A into a ball mill for ball milling to fully mix the two and obtain a mixed material powder;
[0011] Step C, placing the mixed material powder obtained in step B into a quartz boat, then placing the quartz boat into a microwave sintering furnace, sealing the microwave sintering furnace, and then evacuating it;
[0012] Step D: Fill the microwave sintering furnace after vacuuming in step C with nitrogen, and then perform microwave heating with a microwave power of 100 W to make the temperature in the microwave sintering furnace reach 550-650° C. and calcine for 2-4 hours to obtain a dark blue calcined product, which is vanadium dioxide powder.
[0013] Preferably, the method further comprises:
[0014] Step E: When the temperature in the microwave sintering furnace of step D drops to room temperature, the microwave sintering furnace is vented and the quartz boat is taken out;
[0015] Step F: Dry the quartz boat at 60-120° C. and take out the dark blue powder, which is the final product, vanadium dioxide powder.
[0016] The principles of this application are as follows:
[0017] The present invention utilizes equal molar amounts of high-purity ammonium metavanadate and high-purity vanadium pentoxide. Under high temperature conditions, the ammonium metavanadate decomposes to produce hydrogen, nitrogen, and vanadium pentoxide. The resulting hydrogen reduces all vanadium pentoxide in the system, converting it into vanadium dioxide, while also producing water. The nitrogen is then transferred to an inert atmosphere. This process only requires the addition of raw materials, eliminating the need for a separate reducing agent. This simplifies the vanadium dioxide production process, reduces operating costs, and is environmentally friendly.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. The invention of this application is to use the hydrogen generated by the decomposition of ammonium metavanadate to directly reduce all vanadium pentoxide in the system, thereby converting it into vanadium dioxide and generating water. This fully utilizes the raw materials and converts them all into products, achieving high utilization efficiency.
[0020] 2. Advantages of the present invention The process is simple, easy to operate, and no additional reducing agent is required.
[0021] 3. The nitrogen generated by the reaction system can be directly discharged. This process has the characteristics of short process, low material cost, low operating cost, and environmental friendliness, and is suitable for large-scale industrial production. DETAILED DESCRIPTION
[0022] The present invention is described below with reference to specific examples, but the embodiments of the present invention are not limited thereto. Experimental methods in the examples where specific conditions are not specified generally follow conventional conditions, conditions described in manuals, or conditions recommended by the manufacturer. The general equipment, materials, and reagents used are all commercially available unless otherwise specified. The raw materials required in the following examples and comparative examples are all commercially available.
[0023] The "ranges" disclosed herein are defined in terms of lower and upper limits, where a given range is defined by selecting a lower limit and an upper limit, and the selected lower and upper limits define the boundaries of the particular range. Ranges defined in this manner can be inclusive or exclusive of the end values and can be combined arbitrarily, i.e., any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60 to 120 and 80 to 110 are listed for a particular parameter, it is understood that ranges of 60 to 110 and 80 to 120 are also contemplated. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, the following ranges are all contemplated: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4, and 2 to 5. In this application, unless otherwise indicated, the numerical range "a to b" is a shorthand representation of any combination of real numbers between a and b, where a and b are both real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0024] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution. Unless otherwise specified, all technical features and optional technical features of the present application can be combined with each other to form a new technical solution. Unless otherwise specified, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, it is mentioned that the method may also include step (c), which means that step (c) can be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0025] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0026] If not otherwise specified, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B".
[0027] In the following examples, the purity of high-purity ammonium metavanadate is not less than 99.95%, and the purity of high-purity vanadium pentoxide is above 99.9%.
[0028] Example 1
[0029] A method for preparing vanadium dioxide powder comprises the following steps:
[0030] 1. Add equal molar amounts of high-purity ammonium metavanadate and high-purity vanadium pentoxide to a beaker (0.2 mol for each). Stir with a glass rod to mix thoroughly.
[0031] 2. Then put the obtained mixed material into a ball mill for ball milling to fully mix the two and obtain the mixed material powder.
[0032] 3. Put the obtained mixed material powder into a quartz boat, then put the quartz boat into a microwave sintering furnace, seal the microwave sintering furnace, and then evacuate it.
[0033] 4. Fill the vacuumed microwave sintering furnace with high-purity nitrogen and then perform microwave heating at a microwave power of 100 W. When the temperature in the microwave sintering furnace reaches 550°C, sinter for 4 hours to obtain a dark blue sintered product.
[0034] 5. When the temperature in the microwave sintering furnace drops to room temperature, vent the microwave sintering furnace and take out the quartz boat.
[0035] 6. Dry the quartz boat at 120°C and take out the dark blue powder, which is the final product, high-purity vanadium dioxide.
[0036] The overall reaction equation of the above process is as follows:
[0037] 2NH4VO3+2V2O5=N2+6VO2+4H2O
[0038] Example 2
[0039] A method for preparing vanadium dioxide powder comprises the following steps:
[0040] 1. Add equal molar amounts of high-purity ammonium metavanadate and high-purity vanadium pentoxide to a beaker (0.1 mol for each). Stir with a glass rod to mix thoroughly.
[0041] 2. Then put the obtained mixed material into a ball mill for ball milling to fully mix the two and obtain the mixed material powder.
[0042] 3. Put the obtained mixed material powder into a quartz boat, then put the quartz boat into a microwave sintering furnace, seal the microwave sintering furnace, and then evacuate it.
[0043] 4. Fill the vacuumed microwave sintering furnace with high-purity nitrogen and then perform microwave heating at a microwave power of 100 W. When the temperature in the microwave sintering furnace reaches 650°C, sinter for 2 hours to obtain a dark blue sintered product.
[0044] 5. When the temperature in the microwave sintering furnace drops to room temperature, vent the microwave sintering furnace and take out the quartz boat.
[0045] 6. Dry the quartz boat at 60°C and take out the dark blue powder, which is the final product, high-purity vanadium dioxide.
[0046] Comparative Example 1
[0047] The only difference from Example 1 is that high-purity vanadium pentoxide is not added. After the reaction is completed, it is found that all the high-purity ammonium metavanadate is reduced to vanadium trioxide.
[0048] The specific steps are:
[0049] 1. Weigh 0.2 mol of high-purity ammonium metavanadate and place it in a ball mill for ball milling to obtain material powder.
[0050] 2. Put the obtained material powder into a quartz boat, then put the quartz boat into a microwave sintering furnace, seal the microwave sintering furnace, and then evacuate it.
[0051] 3. Fill the vacuumed microwave sintering furnace with high-purity nitrogen and then perform microwave heating at a microwave power of 100 W. When the temperature in the microwave sintering furnace reaches 550° C., sinter for 4 h to obtain a gray-black sintered product.
[0052] 4. When the temperature in the microwave sintering furnace drops to room temperature, vent the microwave sintering furnace and take out the quartz boat.
[0053] 5. Dry the quartz boat at 120°C and take out the gray-black powder, which is the final product, high-purity vanadium trioxide.
[0054] The overall reaction equation of the above process is as follows:
[0055] 2NH4VO3=V2O3+N2+H2+3H2O。
Claims
1. A method for preparing vanadium dioxide powder, characterized in that: The following steps are involved: The same mole number of ammonium metavanadate and vanadium pentoxide are mixed and ball-milled, and calcined at 550-650° C. for 2-4 hours under an inert atmosphere to obtain vanadium dioxide powder.
2. The method for preparing vanadium dioxide powder according to claim 1, characterized in that: The inert atmosphere is nitrogen, helium, neon, argon, krypton or xenon.
3. The method for preparing vanadium dioxide powder according to claim 1, characterized in that: The specific steps include: Step A, adding the same mole number of ammonium metavanadate and vanadium pentoxide into a container, stirring to mix them evenly; Step B, placing the mixed material obtained in step A into a ball mill for ball milling to fully mix the two and obtain a mixed material powder; Step C, placing the mixed material powder obtained in step B into a quartz boat, then placing the quartz boat into a microwave sintering furnace, sealing the microwave sintering furnace, and then evacuating it; Step D: fill the microwave sintering furnace after evacuation in step C with nitrogen, and then perform microwave heating with a microwave power of 100 W, so that the temperature in the microwave sintering furnace reaches 550-650° C., and calcine for 2-4 hours to obtain a dark blue calcined product, which is vanadium dioxide powder.
4. The method for preparing vanadium dioxide powder according to claim 3, characterized in that: The method further comprises: Step E: When the temperature in the microwave sintering furnace of step D drops to room temperature, the microwave sintering furnace is vented and the quartz boat is taken out; Step F, drying the quartz boat at 60-120° C., taking out the dark blue powder therein, which is the final product, vanadium dioxide powder.