Foam concrete foaming agent and application thereof

Through the use of multi-component polymer composite foaming agent, the performance of foam liquid film and cement slurry is optimized, and the stability and physical characteristics of foam concrete in the prior art are solved, thus achieving low water absorption, high fluidity and Strength adjustability, suitable for highway engineering and building materials production.

CN119080434APending Publication Date: 2024-12-06ZHEJIANG COMMUNICATIONS CONSTRUCTION NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411237709.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During the use of existing foam concrete foaming agent, there are problems such as uneven foam distribution, poor stability, high water absorption, low mechanical strength, easy settlement and collapse, easy layering and poor pumping, which cannot meet the foam concrete in highway projects. The physical properties of the product are required, especially in winter, gels are easily formed and foam cannot be produced.

Method used

Using multi-component polymer composite foaming agent, including foaming component A and adjusting component B, foaming component A is made by raw materials such as anionic surfactant, detergent alcohol and glycol ether, water-based bentonite is added The raw materials such as thick rheological agent and silicone leveling agent are made into adjusting component B, combined with the foam stabilized component C, optimize the performance of the foam liquid film and cement slurry to ensure the low water absorption, high fluidity and strength of foam concrete. Adjustability.

Benefits of technology

The foam concrete has achieved low water absorption, high fluidity, adjustability in strength, and is not easy to settle and collapse, meeting the physical characteristics requirements in highway engineering, and maintaining stability in winter to avoid gel phenomenon.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a foam concrete foaming agent and application thereof, the foaming agent comprises a foaming component A and an adjusting component B, and the weight ratio of the foaming component A to the adjusting component B is (0.10-0.15): (1.00-3.00); the foaming component A is prepared from the following raw materials in parts by weight: 15.0-20.0 parts of an anionic surfactant, 2.5-5.0 parts of detergent alcohol, 7.5-12.5 parts of glycol ether and the balance of water, and the total weight is 100 parts; the adjusting component B is prepared from the following raw materials in parts by weight: 40.0-50.0 parts of a water-based bentonite thickening rheological agent, 2.0-5.0 parts of an organic silicon flatting agent and the balance of water, and the total weight is 100 parts; the invention also discloses application of the foam concrete foaming agent in foam concrete. According to the foaming agent disclosed by the invention, the foaming component A and the adjusting component B are adopted to respectively optimize the performance of foam and cement paste which form important components in foam concrete, and the foam stabilizing component C is supplemented to reinforce the performance, so that the foam concrete is low in water absorption, high in fluidity, adjustable in strength, not easy to settle and collapse and low in bleeding amount; the special physical property requirements of the foam concrete in highway engineering construction are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of foam concrete, in particular to a foam concrete foaming agent and application thereof. Background Art

[0002] Foamed concrete is a new type of lightweight thermal insulation material containing a large number of closed pores, which is formed by mechanically foaming the foaming agent through the foaming system of the foaming machine, and uniformly mixing the foam with cement paste, and then pouring it into a cast-in-place or molded through the pumping system of the foaming machine, and then naturally curing it. Foamed concrete is a bubble-like thermal insulation material, and its outstanding feature is that it forms closed foam pores inside the concrete, making the concrete lightweight and thermally insulated. Therefore, it has the advantages of lightness, durability, good self-sustainability, and convenient on-site pouring. It has been widely used in the field of highway engineering, including soft soil foundation treatment, landslide roadbed filling, landslide backfilling, and bridge abutment backfilling. It is also suitable for roof insulation slope sizing, ground insulation cushion and wall pouring, and as a building material such as lightweight foamed concrete bricks.

[0003] In highway construction, foamed concrete must meet specific physical property requirements. For example, its mechanical strength is adjustable, ranging from 0.3 to 5.0 MPa; it has high fluidity and can be transported over long distances of 100 m in vertical height and 500 m in horizontal distance through pipeline pumping; it has good waterproof performance, relatively independent closed bubbles and good integrity, and its volume water absorption rate is less than 15%. In order to meet the requirements of different mechanical strengths, it is necessary to ensure the applicability of a variety of component materials, including different types of cement, added aggregates, fly ash and other fillers. However, existing foaming agents have problems such as poor foaming stability and insufficient foam fineness, which affect the overall performance of foamed concrete.

[0004] The Chinese patent with authorization announcement number CN105948650B discloses a method for preparing a protein-based cement foaming agent, which is carried out according to the following steps: (1) adding 6 to 9 parts of dry leather scraps, 60 to 90 parts of water, 0.4 to 1.2 parts of alkali and 0.4 to 1.2 parts of 2,3-dihydroxynaphthalene-6-sulfonate sodium to a reactor, the reaction temperature is 70 to 100°C, the reaction time is 6 to 12 hours, after the reaction is completed, centrifugation and filtration are performed to obtain leather scrap hydrolyzate and chromium-containing leather scrap hydrolyzate residue; (2) adjusting the pH of the leather scrap hydrolyzate to 6.5 to 7.5, adding 0.01 to 0.5 parts of a preservative to obtain a protein-based foaming agent mother liquor; (3) adding 0.2 to 0.9 parts of a foaming component Q1 and 0.2 to 0.9 parts of a preservative to the protein-based foaming agent mother liquor obtained in step (2) The foaming component Q2 is prepared to obtain a foaming agent mother liquor; (4) adding 0.2 to 0.9 parts of a foam stabilizing component W1 and 0.1 parts of methyltriethoxysilane to the foaming agent mother liquor obtained in step (3) to obtain a protein-type cement foaming agent; the foaming component Q1 is one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium hexadecyl sulfonate, sodium dodecyl polyoxyethylene ether sulfate, and oxidized paraffin soap; the foaming component Q2 is one of sodium dodecyl sulfonate, sodium dodecyl alcohol ether sulfate, tea saponin, and α-oleic acid sulfonate; the foam stabilizing component W1 is one of carboxymethyl cellulose, hydroxyethyl methyl cellulose, hydroxyethyl cellulose, carboxymethyl starch, soluble starch, cationic starch, polyacrylamide, sodium acrylate, sodium alginate, polyvinyl alcohol, polyethylene oxide, and methyl cellulose ether.

[0005] The above-mentioned prior art solutions have the following defects: the above-mentioned foaming agent often has the phenomenon of uneven foam distribution during use, which directly affects the stability and overall performance of the foamed concrete, and then causes the foamed concrete to have problems such as easy perforation, high water absorption, low mechanical strength, easy sedimentation, easy collapse, easy stratification, and poor pumpability, which cannot meet the physical property requirements of foamed concrete in highway engineering construction, especially the protein-type foaming agent is significantly affected by temperature, and it is easy to form gel in winter and cannot produce foam. In order to meet the special requirements of foamed concrete in highway engineering, it is urgent to develop a new type of foamed concrete foaming agent for highway engineering. This new foaming agent should have the characteristics of uniform foam distribution, strong stability, low water absorption, high mechanical strength, not easy to settle and collapse, no stratification and good pumpability, so as to ensure the application effect and service life of foamed concrete in highway engineering. Summary of the invention

[0006] In view of the shortcomings of the prior art, the first purpose of the present invention is to provide a foam concrete foaming agent, which adopts a multi-component polymer composite foaming agent for use in highway engineering construction, and has the advantages of ensuring low water absorption, high fluidity, adjustable strength, not easy to settle and collapse, and low water seepage of foam concrete.

[0007] The second object of the present invention is to provide an application of a foam concrete foaming agent, which has the advantage of good construction performance and is suitable for soft soil foundation treatment, landslide roadbed filling, landslide backfilling and bridge abutment backfilling in highway engineering. It can also be used in construction projects such as roof insulation slope finding, ground insulation cushion and wall pouring, as well as the production of building materials such as lightweight foam concrete bricks.

[0008] To achieve the above first object, the present invention provides the following technical solutions: A foam concrete foaming agent comprises a foaming component A and a regulating component B, wherein the weight ratio of the foaming component A to the regulating component B is 0.10-0.15:1.00-3.00; the foaming component A is prepared from the following raw materials in parts by weight: 15.0-20.0 parts of anionic surfactant, 2.5-5.0 parts of detergent alcohol, 7.5-12.5 parts of glycol ether, and water is added to 100 parts; the regulating component B is prepared from the following raw materials in parts by weight: 40.0-50.0 parts of water-based bentonite thickening rheological agent, 2.0-5.0 parts of organosilicon leveling agent, and water is added to 100 parts.

[0009] By adopting the above technical scheme, in the foaming component A, anionic surfactant is used as the basic foaming component, and low HLB hydrophobic component detergent alcohol and thickening component diol ether are compounded, so that the foam liquid film viscosity is thickened and enhanced, the foam stability is high and the life is long, it is not easy to break and defoam in the cement paste, and the pores are independently closed. Low water absorption of foamed concrete is achieved, and then the pores of foamed concrete are stable and uniform, without sedimentation, collapse, shrinkage, water absorption, and water storage, so it has good mechanical strength and water permeability resistance; in the regulating component B, the water-based bentonite thickening rheological agent can significantly improve the colloidal dispersibility, suspension, and thixotropy of the cement paste, so that Cement paste has good anti-sinking properties and meets the applicability of other materials such as compound aggregates, ensuring that the foamed concrete in highway construction does not sink or collapse, and also achieves adjustability of mechanical strength. Polyether-modified siloxane can reduce the surface tension of cement paste and improve its anti-adhesion properties, promote the leveling and fluidity of cement paste, and meet the requirements of long-distance transportation with a vertical height of 100m and a horizontal distance of 500m by pipeline pumping. In summary, the foaming agent uses foaming component A and regulating component B to optimize the performance of foam and cement paste, which are important components in foamed concrete, respectively, to meet the unique physical property requirements of foamed concrete in highway construction.

[0010] Furthermore, the anionic surfactant is a combination of at least two of sodium α-olefin sulfonate, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, and sodium fatty alcohol polyoxyethylene ether sulfate.

[0011] Furthermore, the anionic surfactant is sodium sulfate of fatty alcohol polyoxyethylene ether and sodium α-olefin sulfonate, sodium sulfate of fatty alcohol polyoxyethylene ether and sodium dodecyl sulfate, or sodium sulfate of fatty alcohol polyoxyethylene ether and sodium dodecylbenzene sulfonate, wherein the sodium α-olefin sulfonate, sodium dodecyl sulfate or sodium dodecylbenzene sulfonate accounts for 20-30% of the total weight of the sodium sulfate of fatty alcohol polyoxyethylene ether. By compounding sodium sulfate of fatty alcohol polyoxyethylene ether and other anionic surfactants and optimizing the compounding ratio, the stability of the foam liquid film can be further enhanced.

[0012] Further, the detergent alcohol is C 12 ~C 14 Mixed alcohols. These detergent alcohols have good hydrophilic-lipophilic balance characteristics, which can further enhance the stability of the foam liquid film and improve the freeze-thaw resistance of foamed concrete.

[0013] Furthermore, the glycol ether is one or a combination of propylene glycol methyl ether, propylene glycol butyl ether, ethylene glycol butyl ether, and diethylene glycol butyl ether. These glycol ethers can effectively reduce the surface tension of the foam liquid film, thereby improving the generation efficiency and stability of the foam.

[0014] Furthermore, the preparation process of the foaming component A includes sequentially adding 15.0-20.0 parts of anionic surfactant, 2.5-5.0 parts of detergent alcohol, and 7.5-12.5 parts of glycol ether into a mixing container, stirring and mixing them evenly, heating to 50-70° C., adding water to 100 parts, and continuing to stir until a clear liquid is formed to obtain the foaming component A.

[0015] Furthermore, the aqueous bentonite thickening rheological agent comprises one or more of nano-modified high-purity sodium-based montmorillonite clay, organically modified hectorite clay, and montmorillonite clay containing active sodium. By using these modified montmorillonite clays to form aqueous bentonite, the viscosity and thixotropy of cement paste can be significantly improved, thereby effectively preventing the sedimentation and collapse of foamed concrete during construction.

[0016] Furthermore, the aqueous bentonite thickening rheological agent is one or a combination of several of Fenghong SMP-N aqueous thickening rheological agent, Hemmingsdeqian BENTONE LT aqueous rheological additive, and Qinghong W200 thickening rheological agent.

[0017] Furthermore, the organosilicon leveling agent comprises one or more of polyether-modified organosilicon, polyether-modified siloxane, and polyether-siloxane copolymer. These organosilicon leveling agents can significantly reduce the surface tension of cement paste, improve its anti-adhesion property, and thus improve the leveling property and fluidity of cement paste.

[0018] Furthermore, the organosilicon leveling agent is one or a combination of the following: KYC-6662 leveling agent from Keying, BYK-333 leveling agent from BYK, and HY-6086 wetting agent from Maier Chemical.

[0019] Furthermore, the preparation process of the regulating component B includes sequentially adding 40.0-50.0 parts of an aqueous bentonite thickening rheological agent and 2.0-5.0 parts of an organosilicon leveling agent into a mixing container, stirring and mixing them evenly, adding water to 100 parts, and continuing to stir until a uniform slurry is formed to obtain the regulating component B.

[0020] Furthermore, it also includes a foam stabilizing component C, wherein the weight ratio of the foaming component A, the regulating component B and the foam stabilizing component C is 0.10-0.15:1.00-3.00:0.40-0.60; the foam stabilizing component C is made of the following raw materials in parts by weight: 10.0-15.0 parts of decyl glucoside, 1.0-3.0 parts of corn starch, 0.1-0.3 parts of menthol, 0.5-1.0 parts of dimethyl glycyrrhizinate, 0.8-1.5 parts of oleanolic acid, and water is added to 100 parts.

[0021] In the foam-stabilizing component C, decyl glucoside is a new type of nonionic surfactant APG, which has the characteristics of ordinary nonionic and anionic surfactants. When used in combination with anionic surfactants and corn starch, it can improve the hard water resistance of anionic surfactants while the three can form a more stable foam structure in foam concrete. The hydrophilic-lipophilic balance property enables decyl glucoside to better combine with other components in the cement paste, and corn starch, as a natural polymer material, can further enhance the adhesion and compressive strength of the foam, thereby improving the stability and durability of the foam; at the same time, menthol reduces the surface tension of the liquid on the foam surface and promotes the formation of bubbles. Glycyrrhizic acid dimethyl and oleanol work synergistically to enhance the defense ability of the foam liquid film, thereby effectively resisting external pressure and impact, and further ensuring the stability and durability of the foam structure.

[0022] Furthermore, the preparation process of the foam stabilizing component C includes sequentially adding 10.0-15.0 parts of decyl glucoside, 1.0-3.0 parts of corn starch, 0.1-0.3 parts of menthol, 0.5-1.0 parts of dimethyl glycyrrhizinate, and 0.8-1.5 parts of oleanolic acid into a mixing container, stirring and mixing evenly, adding water to 100 parts, and continuing to stir until a uniform slurry is formed to obtain the foam stabilizing component C.

[0023] To achieve the above second purpose, the present invention provides the following technical solutions: A foam concrete foaming agent is used in foam concrete. The preparation process of the foam concrete comprises: S1 diluting the foaming component A with water by 50 to 60 times to obtain a foaming solution; S2: 365-410 parts of cement and 231-246 parts of water are sequentially put into a mixing container, and a regulating component B accounting for 1.0-3.0% of the total weight of cement and a foam stabilizing component C accounting for 0.40-0.60% of the total weight of cement are added, and the mixture is stirred and mixed to obtain cement paste; S3 forms a predetermined foam through a foaming machine on the foaming solution obtained in S1, and then forcibly presses the foaming solution into the cement paste obtained in S2, and controls the mass ratio of the cement to the foaming component A to be 365-410:0.45-0.55, and continues to stir and mix evenly to obtain foamed concrete.

[0024] By adopting the above technical solution, the effective application of the foam concrete foaming agent in highway engineering construction can be ensured, and the physical property requirements of the foam concrete such as low water absorption, high fluidity, adjustable strength, not easy to settle and collapse, and low water seepage can be met. In addition, when the foam concrete foaming agent of the present invention is used in winter, due to its unique formula design, it can effectively avoid the gel phenomenon caused by temperature changes, thereby ensuring the stability and construction performance of the foam concrete in a low temperature environment.

[0025] In summary, the beneficial technical effects of the present invention are: 1. The foaming agent of the present invention uses a foaming component A and a regulating component B to optimize the performance of foam and cement paste, which are important components in the foamed concrete, respectively, and uses a foam stabilizing component C to enhance the performance, thereby ensuring low water absorption, high fluidity, adjustable strength, low sedimentation and collapse, and low water seepage of the foamed concrete, meeting the unique physical property requirements of the foamed concrete in highway engineering construction; 2. The foaming agent of the present invention can be applied to foam concrete, and is suitable for soft soil foundation treatment, landslide roadbed filling, landslide backfilling, and bridge abutment backfilling in highway engineering. It can also be used in roof insulation slope finding, ground insulation cushion and wall pouring and other construction projects, as well as the production of building materials such as lightweight foam concrete bricks. DETAILED DESCRIPTION

[0026] In order to make the technical means, creative features, objectives and functions achieved by the present invention clearer and easier to understand, the present invention is further explained below in conjunction with specific implementation methods.

[0027] Embodiment 1: A foam concrete foaming agent disclosed in the present invention comprises a foaming component A, a regulating component B and a foam stabilizing component C. The specific implementation method of each component in the foaming agent is as follows: S1: 15.0 parts of anionic surfactant, 2.5 parts of detergent alcohol, and 7.5 parts of glycol ether are sequentially put into a mixing container, stirred and mixed evenly, heated to 60°C, and water is added to 100 parts, and stirred continuously until a clear liquid is formed to obtain a foaming component A; The anionic surfactant is 12.5 parts of sodium fatty alcohol polyoxyethylene ether sulfate and 4.5 parts of sodium α-olefin sulfonate; Detergent alcohol is C 12 ~C 14 Mixed alcohols; The glycol ethers are 0 parts of propylene glycol methyl ether, 7.5 parts of propylene glycol butyl ether, 0 parts of ethylene glycol butyl ether, and 0 parts of diethylene glycol butyl ether; S2: 40.0 parts of aqueous bentonite thickening rheological agent and 3.5 parts of silicone leveling agent are sequentially added into a mixing container, stirred and mixed evenly, and then water is added to 100 parts, and stirring is continued until a uniform slurry is formed to obtain a regulating component B; wherein, The bentonite thickening rheological agent is Fenghong SMP-N water-based thickening rheological agent; The organic silicon leveling agent is Keying KYC-6662 leveling agent; S3: 10.0 parts of decyl glucoside, 3.0 parts of corn starch, 0.2 parts of menthol, 0.5 parts of dimethyl glycyrrhizinate, and 1.2 parts of oleanolic acid are sequentially put into a mixing container, stirred and mixed evenly, and then water is added to 100 parts, and stirring is continued until a uniform slurry is formed to obtain a foam stabilizing component C.

[0028] The invention also discloses an application of a foam concrete foaming agent in foam concrete. The preparation process of the foam concrete includes: S1 dilute the foaming component A with water 50 times to obtain a foaming solution; S2: 365 parts of cement and 231 parts of water are sequentially put into a mixing container, and a regulating component B accounting for 3.0% of the total weight of cement and a foam stabilizing component C accounting for 0.40% of the total weight of cement are added, and the mixture is stirred and mixed to obtain cement paste; S3 passes the foaming solution prepared in S1 through a foaming machine (JH-300) to form a predetermined foam, and then forcibly presses it into the cement paste prepared in S2, and controls the mass ratio of cement to foaming component A to be 365:0.55, and continues to stir and mix evenly to obtain foamed concrete.

[0029] Embodiment 2: A foam concrete foaming agent disclosed in the present invention comprises a foaming component A, a regulating component B and a foam stabilizing component C. The specific implementation method of each component in the foaming agent is as follows: S1: 19.5 parts of anionic surfactant, 3.5 parts of detergent alcohol, and 10 parts of glycol ether are sequentially put into a mixing container, stirred and mixed evenly, heated to 60°C, and water is added to 100 parts, and stirred continuously until a clear liquid is formed to obtain a foaming component A; The anionic surfactant is 15.0 parts of sodium fatty alcohol polyoxyethylene ether sulfate and 3.5 parts of sodium lauryl sulfate; Detergent alcohol is C 12 ~C 14 Mixed alcohols; The glycol ethers are 0 parts of propylene glycol methyl ether, 0 parts of propylene glycol butyl ether, 7.5 parts of ethylene glycol butyl ether, and 2.5 parts of diethylene glycol butyl ether; S2: 45.0 parts of aqueous bentonite thickening rheological agent and 2.0 parts of silicone leveling agent are sequentially added into a mixing container, stirred and mixed evenly, and then water is added to 100 parts, and stirring is continued until a uniform slurry is formed to obtain a regulating component B; wherein, The bentonite thickening rheological agent is Hemmingsdeqian BENTONE LT water-based rheological additive; The silicone leveling agent is BYK-333 leveling agent; S3: 12.5 parts of decyl glucoside, 2.0 parts of corn starch, 0.3 parts of menthol, 1.0 parts of dimethyl glycyrrhizinate, and 0.8 parts of oleanolic acid are sequentially put into a mixing container, stirred and mixed evenly, and then water is added to 100 parts, and stirring is continued until a uniform slurry is formed to obtain a foam stabilizing component C.

[0030] The invention also discloses an application of a foam concrete foaming agent in foam concrete. The preparation process of the foam concrete includes: S1 dilute the foaming component A with water 55 times to obtain a foaming solution; S2: 385 parts of cement and 231 parts of water are sequentially put into a mixing container, and a regulating component B accounting for 2.0% of the total weight of cement and a foam stabilizing component C accounting for 0.50% of the total weight of cement are added, and the mixture is stirred and mixed to obtain a cement paste; S3 passes the foaming solution prepared in S1 through a foaming machine (JH-300) to form a predetermined foam, and then forcibly presses it into the cement paste prepared in S2, and controls the mass ratio of cement to foaming component A to be 385:0.50, and continues to stir and mix evenly to obtain foamed concrete.

[0031] Embodiment 3: A foam concrete foaming agent disclosed in the present invention comprises a foaming component A, a regulating component B and a foam stabilizing component C. The specific implementation method of each component in the foaming agent is as follows: S1: 17.5 parts of anionic surfactant, 5.0 parts of detergent alcohol, and 12.5 parts of glycol ether are sequentially put into a mixing container, stirred and mixed evenly, heated to 60°C, and water is added to 100 parts, and stirred continuously until a clear liquid is formed to obtain a foaming component A; The anionic surfactant is 14.0 parts of sodium fatty alcohol polyoxyethylene ether sulfate and 4.5 parts of sodium dodecylbenzene sulfonate; Detergent alcohol is C 12 ~C 14 Mixed alcohols; The glycol ether is 7.5 parts of propylene glycol methyl ether, 0 parts of propylene glycol butyl ether, 5 parts of ethylene glycol butyl ether, and 0 parts of diethylene glycol butyl ether; S2: 50.0 parts of aqueous bentonite thickening rheological agent and 5.0 parts of silicone leveling agent are sequentially added into a mixing container, stirred and mixed evenly, and then water is added to 100 parts, and stirring is continued until a uniform slurry is formed to obtain a regulating component B; wherein, The bentonite thickening rheological agent is Qinghong W200 thickening rheological agent; The silicone leveling agent is Maier Chemical HY-6086 wetting agent; S3: 15.0 parts of decyl glucoside, 1.0 part of corn starch, 0.1 part of menthol, 0.8 parts of dimethyl glycyrrhizinate, and 1.5 parts of oleanolic acid are sequentially put into a mixing container, stirred and mixed evenly, and then water is added to 100 parts, and stirring is continued until a uniform slurry is formed to obtain a foam stabilizing component C.

[0032] The invention also discloses an application of a foam concrete foaming agent in foam concrete. The preparation process of the foam concrete includes: S1 dilute the foaming component A with water 60 times to obtain a foaming solution; S2: 410 parts of cement and 246 parts of water are sequentially put into a mixing container, and a regulating component B accounting for 1.0% of the total weight of cement and a foam stabilizing component C accounting for 0.60% of the total weight of cement are added, and the mixture is stirred and mixed to obtain cement paste; S3 passes the foaming solution prepared in S1 through a foaming machine (JH-300) to form a predetermined foam, and then forcibly presses it into the cement paste prepared in S2, and controls the mass ratio of cement to foaming component A to be 410:0.45, and continues to stir and mix evenly to obtain foamed concrete.

[0033] Comparative Examples 1 to 3 are a foam concrete foaming agent and application thereof disclosed in the present invention, which are different from Example 1 in that the detergent alcohol and glycol ether in the foaming component A are not used.

[0034] Comparative Examples 4 to 6 are foam concrete foaming agents and applications thereof disclosed in the present invention, which are different from Example 1 in that the regulating component B is not used.

[0035] Comparative Examples 7 to 9 are foam concrete foaming agents and applications thereof disclosed in the present invention, which are different from Example 1 in that the foam stabilizing component C is not used.

[0036] Test example 1: According to the relevant test methods in CJJ / T 177-2012 "Technical Code for Bubble Mixed Lightweight Soil Filling Engineering", the water seepage, settlement distance, fluidity, water absorption rate and compressive strength of the foamed concrete of Examples 1 to 3 and Comparative Examples 1 to 9 were tested, and the results are shown in Table 1.

[0037] Table 1 Group Foam density / kg / m³ Water secretion / mL Settlement distance / mm Fluidity / mm Water absorption / % 28d compressive strength / MPa Example 1 45 20 1.8 192 13 4.5 Comparative Example 1 45 32 3.5 171 25 3.0 Comparative Example 4 45 46 4.8 144 19 2.8 Comparative Example 7 45 36 3.6 132 39 2.9 Example 2 47 22 2.1 193 10 4.8 Comparative Example 2 47 45 4.2 146 24 3.4 Comparative Example 5 47 50 5.1 174 38 3.1 Comparative Example 8 47 39 3.9 173 18 3.2 Example 3 50 23 2.4 194 12 5.2 Comparative Example 3 50 38 4.8 172 26 3.7 Comparative Example 6 50 54 6.4 168 19 3.5 Comparative Example 9 50 41 4.0 142 42 3.8 From Table 1, we can see that In the foaming component A, anionic surfactant is used as the basic foaming component, and low HLB hydrophobic component detergent alcohol and thickening component glycol ether are compounded, so that the foam liquid film viscosity is thickened and enhanced, the foam stability is high and the life is long, it is not easy to break and defoam in the cement paste, and the pores are independently closed. Low water absorption of the foamed concrete is achieved, and then the pores of the foamed concrete are stable and uniform, and do not sink, collapse, shrink, absorb water, or store water, so it has good mechanical strength and water resistance; In the adjustment component B, the water-based bentonite thickening rheological agent can significantly improve the colloidal dispersion, suspension and thixotropy of the cement paste, so that the cement paste has good anti-settling properties and meets the applicability of other materials such as compound aggregates, ensuring that the foamed concrete in highway construction does not sink or collapse, and also achieves the adjustability of mechanical strength. The polyether-modified siloxane can reduce the surface tension of the cement paste and improve its anti-adhesion properties, promote the leveling and fluidity of the cement paste, and meet the requirements of long-distance transportation with a vertical height of 100m and a horizontal distance of 500m for pipeline pumping. Furthermore, in the foam-stabilizing component C, decyl glucoside is a new type of nonionic surfactant APG, which has the characteristics of both common nonionic and anionic surfactants. When used in combination with anionic surfactants and corn starch, it can improve the hard water resistance of anionic surfactants while forming a more stable foam structure in foamed concrete. The hydrophilic-lipophilic balance property enables decyl glucoside to better combine with other components in cement paste, while corn starch, as a natural polymer material, can further enhance the adhesion and compressive strength of foam, thereby improving the stability and durability of foam. At the same time, menthol reduces the surface tension of liquid on the foam surface and promotes the formation of bubbles. Dimethyl glycyrrhizinate and oleanol work synergistically to enhance the defense capability of the foam liquid film, thereby effectively resisting external pressure and impact, further ensuring the stability and durability of the foam structure. In summary, the foaming agent of the present invention uses the foaming component A and the regulating component B to respectively optimize the performance of the foam and cement paste, which are important components in the foamed concrete, and uses the foam stabilizing component C to enhance the performance, thereby ensuring the low water absorption, high fluidity, adjustable strength, low sedimentation and collapse, and low water seepage of the foamed concrete, thereby meeting the unique physical property requirements of the foamed concrete in highway engineering construction.

[0038] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A foam concrete foaming agent, characterized in that: The invention comprises a foaming component A and an adjusting component B, wherein the weight ratio of the foaming component A to the adjusting component B is 0.10-0.15:1.00-3.00; the foaming component A is prepared from the following raw materials in parts by weight: 15.0-20.0 parts of anionic surfactant, 2.5-5.0 parts of detergent alcohol, 7.5-12.5 parts of glycol ether, and water is added to 100 parts; the adjusting component B is prepared from the following raw materials in parts by weight: 40.0-50.0 parts of water-based bentonite thickening rheological agent, 2.0-5.0 parts of organosilicon leveling agent, and water is added to 100 parts.

2. A foam concrete foaming agent according to claim 1, characterized in that: The anionic surfactant is a combination of at least two of sodium α-olefin sulfonate, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, and sodium fatty alcohol polyoxyethylene ether sulfate.

3. A foam concrete foaming agent according to claim 1, characterized in that: The anionic surfactant is sodium sulfate of fatty alcohol polyoxyethylene ether and sodium α-olefin sulfonate, sodium sulfate of fatty alcohol polyoxyethylene ether and sodium dodecyl sulfate, or sodium sulfate of fatty alcohol polyoxyethylene ether and sodium dodecylbenzene sulfonate, wherein the sodium α-olefin sulfonate, sodium dodecyl sulfate or sodium dodecylbenzene sulfonate accounts for 20-30% of the total weight of the sodium sulfate of fatty alcohol polyoxyethylene ether.

4. A foam concrete foaming agent according to claim 1, characterized in that: The detergent alcohol is C 12 ~C 14 Mixed alcohols.

5. A foam concrete foaming agent according to claim 1, characterized in that: The diol ether is one or a combination of propylene glycol methyl ether, propylene glycol butyl ether, ethylene glycol butyl ether and diethylene glycol butyl ether.

6. A foam concrete foaming agent according to claim 1, characterized in that: The aqueous bentonite thickening rheological agent comprises one or a combination of nano-modified high-purity sodium-based montmorillonite clay, organically modified hectorite clay, and montmorillonite clay containing active sodium.

7. A foam concrete foaming agent according to claim 1, characterized in that: The organic silicon leveling agent comprises one or a combination of polyether-modified organic silicon, polyether-modified siloxane, and polyether-siloxane copolymer.

8. A foam concrete foaming agent according to claim 6 or 7, characterized in that: The aqueous bentonite thickening rheological agent is one or a combination of Fenghong SMP-N aqueous thickening rheological agent, Hemmingsdeqian BENTONE LT aqueous rheological additive, and Qinghong W200 thickening rheological agent; the silicone leveling agent is one or a combination of Keying KYC-6662 leveling agent, BYK-333 leveling agent, and Maier Chemical HY-6086 wetting agent.

9. A foam concrete foaming agent according to claim 1, characterized in that: It also includes a foam stabilizing component C, wherein the weight ratio of the foaming component A, the regulating component B and the foam stabilizing component C is 0.10-0.15:1.00-3.00:0.40-0.60; the foam stabilizing component C is made of the following raw materials in parts by weight: 10.0-15.0 parts of decyl glucoside, 1.0-3.0 parts of corn starch, 0.1-0.3 parts of menthol, 0.5-1.0 parts of dimethyl glycyrrhizinate, 0.8-1.5 parts of oleanolic acid, and water is added to 100 parts.

10. Use of a foamed concrete foaming agent according to any one of claims 1 to 9 in foamed concrete, characterized in that: The preparation process of the foamed concrete includes: S1 diluting the foaming component A with water by 50 to 60 times to obtain a foaming solution; S2: 365-410 parts of cement and 231-246 parts of water are sequentially put into a mixing container, and a regulating component B accounting for 1.0-3.0% of the total weight of cement and a foam stabilizing component C accounting for 0.40-0.60% of the total weight of cement are added, and the mixture is stirred and mixed to obtain cement paste; S3 forms a predetermined foam through a foaming machine on the foaming solution obtained in S1, and then forcibly presses the foaming solution into the cement paste obtained in S2, and controls the mass ratio of the cement to the foaming component A to be 365-410:0.45-0.55, and continues to stir and mix evenly to obtain foamed concrete.