Solid waste-based guniting material as well as preparation method and application thereof

Through solid waste-based spraying materials without cement, using the combination of active powder and exciter, the high energy consumption and high pollution problems of cement materials in tunnel support are solved, high early strength and good bonding performance are achieved, and high strength and good bonding performance are improved. Solid waste resource utilization rate and reduce costs.

CN119080447APending Publication Date: 2024-12-06JIZHI WISDOM (SHANGHAI) NEW TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411210865.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing spraying materials rely on cement in the support of the tunnel, resulting in high energy consumption, high pollution and high cost, and insufficient compressive strength, making it difficult to effectively utilize industrial waste slag.

Method used

Using solid waste-based spraying materials without cement, by mixing active powders (such as gangue, fly ash, red mud, ore powder, steel slag) with the exciter and stirring them with aggregate and water in a specific proportion. Form sprayed materials with high early strength and bonding properties.

Benefits of technology

It has achieved a green and environmentally friendly production process, fast hardening speed, high early strength, good bonding performance, and improved solid waste resource utilization, reduced costs, and met the compressive strength requirements of 42.5-grade silicate cement.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a solid waste-based guniting material as well as a preparation method and application thereof. The solid waste based guniting material comprises the following components in parts by weight: 70-100 parts of active powder and 5-20 parts of an exciting agent, wherein the active powder is selected from at least two of coal gangue, fly ash, red mud, mineral powder, silica fume and steel slag; the solid waste based guniting material does not contain cement. The solid waste-based guniting material does not contain cement, has the characteristic of green and environment-friendly production process, and is high in hardening speed, high in early strength and good in adhesive property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a solid waste-based shotcrete material and a preparation method and application thereof. Background Art

[0002] Shotcrete is a quick-setting material used to reinforce and protect structures or rock surfaces. The mixture is sprayed onto the working surface with the help of a spraying machine and solidifies in a very short time. It has the functions of reinforcing the shaft wall, plugging the gaps in the wall, and waterproofing and preventing seepage. At present, a large number of shotcrete materials are based on cement concrete. For example, a coal mine with an annual output of 2 million tons has a tunnel construction length of about 3,000 meters per year. The shotcrete used to make tunnel support consumes a large amount of cement and river sand, resulting in high costs. However, my country's cement industry CO 2 Emissions account for 13% of the total national emissions and more than 60% of the national industrial process emissions, causing environmental pollution. On the other hand, among industrial waste residues, fly ash, blast furnace slag and steel slag have high emissions and low utilization rates, causing storage problems and also causing environmental pollution.

[0003] CN116813289A discloses a mine shotcrete material and its use method. The shotcrete material includes 20-70 parts of desulfurized gypsum, 5-30 parts of fly ash, 10-35 parts of cement, 10-50 parts of sand and 0-5 parts of additives. The application contains cement, and the compressive strength needs to be further improved.

[0004] CN113603412A discloses a dry-mixed shotcrete material composition for underground tunnels in coal mines, which includes the following raw materials: 30-60 parts by weight of natural sand, 5-30 parts by weight of machine-made sand, 20-30 parts by weight of fly ash, 0.6-1.0% volume percentage of short fiber material, 150-300 parts by weight of cement, 1-2 parts by weight of defoamer, 3-8 parts by weight of water reducer, and 5-15 parts by weight of quick-setting agent; wherein the machine-made sand is made by crushing construction waste and then coating it. This application still uses cement as the main strength component. Although the compressive strength has been improved to a certain extent, the method is complicated, costly, and not conducive to promotion.

[0005] CN109694231A discloses a phosphate-magnesium-based cement shotcrete material and its preparation method and application. The shotcrete material is made of the following materials in proportion by weight: 40-70 parts of composite magnesium compound, 0.5-3 parts of composite retarder, 0.3-0.8 parts of water reducer, 10-40 parts of phosphate, 0.5-1.5 parts of viscosity enhancer, and 0.3-0.7 parts of fiber. The shotcrete material is weighed in proportion and mixed with sand in a ratio of 1:3, wherein the sand is medium sand or coarse sand: the fine sand is a mixed sand of 4:1, and then the shotcrete material is mixed with sand and then mixed with water in a ratio of 100:15-30 to form a slurry, and the mixture is obtained after being evenly mixed. Although the application does not use cement clinker, the 28d compressive strength is only above 25MPa, which still needs to be further improved. Summary of the invention

[0006] In view of this, one object of the present invention is to provide a solid waste-based shotcrete material, which does not contain cement, has the characteristics of green and environmentally friendly production process, and the shotcrete material has a fast hardening speed, high early strength and good bonding performance. Another object of the present invention is to provide a method for preparing the solid waste-based shotcrete material as described above. Another object of the present invention is to provide an application of the solid waste-based shotcrete material as described above in tunnel and slope protection.

[0007] The above technical objectives are achieved through the following technical solutions.

[0008] On the one hand, the present invention provides a solid waste-based shotcrete material, comprising 70 to 100 parts by weight of active powder and 5 to 20 parts by weight of activator; wherein the active powder is selected from at least two of coal gangue, fly ash, red mud, mineral powder, silica fume, and steel slag; and the solid waste-based shotcrete material does not contain cement.

[0009] The solid waste-based shotcrete material according to the present invention preferably further comprises aggregate and water; wherein the mass of the aggregate is 50 to 400 parts by weight; and the mass of the water is 20 to 55 parts by weight.

[0010] According to the solid waste-based shotcrete material of the present invention, preferably, the active powder comprises the following components: 0 to 30 parts by weight of coal gangue, 0 to 30 parts by weight of fly ash, 0 to 20 parts by weight of red mud, 0 to 50 parts by weight of mineral powder, 0 to 20 parts by weight of silica fume, and 0 to 50 parts by weight of steel slag.

[0011] The solid waste-based shotcrete material according to the present invention is preferably composed of the following components: 2 to 15 parts by weight of coal gangue, 2 to 20 parts by weight of fly ash, 5 to 20 parts by weight of red mud, 10 to 50 parts by weight of mineral powder and 10 to 50 parts by weight of steel slag.

[0012] According to the solid waste-based shotcrete material of the present invention, preferably, the activator is selected from one or more of silicates, aluminates, phosphates, sulfates, carbonates and caustic alkalis.

[0013] According to the solid waste-based shotcrete material of the present invention, preferably, the aggregate is selected from one or more of tailings sand, river sand, river sand and machine-made sand.

[0014] According to the solid waste-based shotcrete material of the present invention, preferably, the particle size of the aggregate is ≤4.75 mm.

[0015] According to the solid waste-based shotcrete material of the present invention, preferably, the solid waste-based shotcrete material has a 3d compressive strength of >20 MPa; a 28d compressive strength of >42.5 MPa; a bonding force of >1.3 MPa; and a consistency of 80-100 mm.

[0016] On the other hand, the present invention provides a method for preparing the solid waste-based shotcrete material as described above, comprising the following steps:

[0017] (1) mixing the active powder and the activator in proportion to obtain a dry mixed solid waste-based spraying material;

[0018] (2) The dry mixed solid waste-based shotcrete material, aggregate and water are mixed and stirred in a ratio of 1:0.5-6:0.2-0.8 to obtain the solid waste-based shotcrete material.

[0019] On the other hand, the present invention also provides the use of the solid waste-based shotcrete material as described above in tunnel and slope protection.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The solid waste-based spraying material of the present application does not contain cement, thus avoiding the high energy consumption and high pollution in cement production, and has the characteristics of green, environmentally friendly and resource-saving production process.

[0022] (2) The solid waste-based spraying material of the present application has a fast hardening speed, high early strength, good bonding performance, suitable consistency and easy meshing, so the rebound rate is small.

[0023] (3) The resource utilization of solid waste is improved, and the raw materials are widely available and of low cost. DETAILED DESCRIPTION

[0024] The present invention is described in more detail below, but the present invention is not limited thereto.

[0025] <Solid waste-based shotcrete materials>

[0026] The solid waste-based spraying material of the present invention is prepared from active powder and an activator. Preferably, it can be prepared from active powder, an activator, aggregate and water.

[0027] In the present invention, the mass of the active powder may be 70 to 100 parts by weight, preferably 80 to 95 parts by weight, and more preferably 85 to 90 parts by weight.

[0028] In the present invention, the active powder can be selected from at least two of coal gangue, fly ash, red mud, mineral powder, silica fume, and steel slag; preferably, it can be selected from at least three of coal gangue, fly ash, red mud, mineral powder, silica fume, and steel slag; more preferably, it can be selected from at least four of coal gangue, fly ash, red mud, mineral powder, silica fume, and steel slag. According to an embodiment of the present invention, the active powder is selected from coal gangue, fly ash, red mud, mineral powder, and steel slag.

[0029] In the present invention, the coal gangue can be selected from aluminum-silicon type coal gangue or calcium-magnesium type coal gangue, preferably aluminum-silicon type coal gangue, and the mass of the coal gangue can be 0 to 30 parts by weight, preferably 2 to 15 parts by weight, and more preferably 5 to 10 parts by weight.

[0030] In the present invention, fly ash can be selected from Class F fly ash in GB / T 1596-2017, preferably Class I fly ash. The mass of fly ash can be 0 to 30 parts by weight, preferably 2 to 20 parts by weight, and more preferably 10 to 18 parts by weight.

[0031] In the present invention, the red mud can be sintered red mud, Bayer red mud or combined red mud, preferably sintered red mud. The mass of the red mud can be 0 to 20 parts by weight, preferably 5 to 20 parts by weight, and more preferably 10 to 18 parts by weight.

[0032] In the present invention, the mineral powder can be selected from the granulated blast furnace slag powder in GB / T 18046-2017, preferably slag powder of grade S95 or above. The mass of the mineral powder can be 0 to 50 parts by weight, preferably 10 to 50 parts by weight, and more preferably 30 to 45 parts by weight.

[0033] In the present invention, the steel slag can be converter steel slag or electric furnace steel slag, preferably steel slag powder after magnetic separation and iron removal, more preferably first-grade steel slag powder. The mass of the steel slag can be 0 to 50 parts by weight, preferably 5 to 50 parts by weight, more preferably 8 to 20 parts by weight.

[0034] In the present invention, the silica fume can be selected from the original silica fume in GB / T 27690-2023, preferably SF90 grade silica fume. The mass of the silica fume can be 0 to 20 parts by weight, preferably 2 to 18 parts by weight, and more preferably 5 to 15 parts by weight.

[0035] In the present invention, the activator can be selected from one or more of silicates, aluminates, phosphates, sulfates, carbonates, and caustic alkalis; preferably selected from one or more of silicates, aluminates, sulfates, and caustic alkalis; more preferably selected from one or more of silicates, sulfates, and caustic alkalis. The mass of the activator can be 5 to 20 parts by weight, preferably 10 to 20 parts by weight, and more preferably 15 to 20 parts by weight.

[0036] In the present invention, the mass of the aggregate may be 50 to 400 parts by weight, preferably 100 to 350 parts by weight, more preferably 150 to 300 parts by weight. The mass of water may be 20 to 55 parts by weight, preferably 30 to 50 parts by weight, more preferably 30 to 45 parts by weight.

[0037] In the present invention, the aggregate can be selected from one or more of tailings sand, river sand, river sand, and machine-made sand, preferably one or more of tailings sand, river sand, or river sand, and more preferably tailings sand. Among them, the tailings sand can be selected from one of iron tailings sand, copper tailings sand, and limestone tailings sand, preferably iron tailings sand or limestone tailings sand, more preferably iron tailings sand, and more preferably iron tailings fine sand with a fineness modulus of 2.2 to 1.6; the mud content of the tailings sand is less than 1%, preferably less than 0.5%; the mud content of the river sand and river sand is less than 1.5%, preferably less than 1%, and more preferably less than 0.5%; the mud content of the river sand and river sand is less than 5%, preferably less than 3%; the stone powder content and mud content of the machine-made sand are both not more than 5%, preferably not more than 3%.

[0038] In the present invention, the particle size of the aggregate may be 4.75 mm or less, preferably 2.5 mm or less, and more preferably 2 mm or less.

[0039] In the present invention, the 3d compressive strength of the solid waste-based shotcrete material is greater than 20 MPa, preferably, the 3d compressive strength is greater than 25 MPa; the 28d compressive strength is greater than 42.5 MPa, preferably, the 28d compressive strength is greater than 45 MPa; the bonding force is greater than 1.3 MPa, preferably, the bonding force is greater than 1.5 MPa, and more preferably, the bonding force is greater than 1.7 MPa; the consistency is 80-100 mm, preferably 80-95 mm.

[0040] <Preparation method of solid waste-based shotcrete material>

[0041] The method for preparing the solid waste-based spraying material of the present invention comprises the following steps:

[0042] (1) uniformly mixing the active powder and the activator in proportion to obtain a dry-mixed solid waste-based spraying material;

[0043] (2) The dry mixed solid waste-based shotcrete material obtained in step (1) is mixed with aggregate and water in proportion to obtain a solid waste-based shotcrete material.

[0044] In the present invention, the mass ratio of the dry-mixed solid waste-based shotcrete material, aggregate and water can be 1:0.5-6:0.2-0.8, preferably 1:1-5:0.25-0.45, and more preferably 1:2-4:0.3-0.4.

[0045] In step (1) of the present invention, the active powder and the stimulant can be mixed by a ribbon mixer, a weightless mixer, a double-helix cone mixer or a planetary mixer, preferably a ribbon mixer or a weightless mixer, more preferably a ribbon mixer, such as a horizontal ribbon mixer.

[0046] In step (2) of the present invention, there is no special regulation on the mixing method, and the mixing method commonly used in the art can be adopted, such as mechanical stirring.

[0047] <Application of solid waste-based shotcrete materials>

[0048] The solid waste-based spraying material of the present invention can be used in tunnel and slope protection, especially in tunnels. The spraying material of the present invention has good bonding performance and suitable consistency for easy meshing, so the rebound rate is small, which can avoid material waste.

[0049] In the following examples, unless otherwise specified, the parts are by weight.

[0050] Example 1

[0051] 5 parts of coal gangue, 5 parts of fly ash, 50 parts of steel slag, 10 parts of red mud, 15 parts of mineral powder and 15 parts of activator are fed into a horizontal ribbon mixer and uniformly mixed to obtain a dry-mixed solid waste-based shotcrete material; wherein the coal gangue is aluminum-silicon type coal gangue; the fly ash is Class I fly ash; the steel slag is Class I steel slag powder; the red mud is sintered red mud; the mineral powder is Class S95 mineral powder; the activator consists of 10 parts of silicate and 5 parts of caustic soda;

[0052] The dry mixed solid waste-based shotcrete material, aggregate and water are fed into a mixer in a ratio of 1:3:0.3, and stirred to obtain the solid waste-based shotcrete material, wherein the aggregate is iron tailings sand.

[0053] Example 2

[0054] 10 parts of coal gangue, 10 parts of fly ash, 10 parts of steel slag, 10 parts of red mud, 45 parts of mineral powder and 15 parts of activator are fed into a horizontal ribbon mixer and uniformly mixed to obtain a dry-mixed solid waste-based shotcrete material; wherein the raw material parameters are the same as those in Example 1; the activator is composed of 5 parts of silicate, 5 parts of sulfate and 5 parts of caustic soda;

[0055] The dry mixed solid waste-based shotcrete material, aggregate and water are fed into a mixer in a ratio of 1:3:0.3, and stirred to obtain the solid waste-based shotcrete material, wherein the aggregate is iron tailings sand.

[0056] Example 3

[0057] 8 parts of coal gangue, 16 parts of fly ash, 8 parts of steel slag, 16 parts of red mud, 32 parts of mineral powder and 20 parts of activator are fed into a horizontal ribbon mixer and uniformly mixed to obtain a dry-mixed solid waste-based shotcrete material; wherein the raw material parameters are the same as those in Example 1; the activator is composed of 5 parts of silicate, 10 parts of sulfate and 5 parts of caustic soda;

[0058] The dry mixed solid waste-based shotcrete material, aggregate and water are fed into a mixer in a ratio of 1:3:0.3, and stirred to obtain the solid waste-based shotcrete material.

[0059] Comparative Example 1

[0060] In this comparative example, except that the steel slag is 45 parts, the activator is 20 parts, and the ratio of dry-mixed solid waste-based shotcrete material, aggregate and water is 1:3:0.5, the rest is the same as Example 1.

[0061] Comparative Example 2

[0062] Except that the ratio of dry-mixed solid waste-based shotcrete material, aggregate and water is 1:3:0.5, the rest is the same as Example 3.

[0063] The solid waste-based shotcrete materials obtained in Examples 1 to 3 and Comparative Examples 1 to 2 were molded in a 70.7×70.7×70.7mm test mold according to the "JGJ / T70-2009 Standard for Basic Performance Test Methods of Building Mortar", and the cubic compressive strength was measured after curing; the consistency was tested using a mortar consistency meter; a 70×70×20mm base mortar specimen was prepared, and a 40×40×6mm bonding strength test specimen was prepared on the molding surface of the base specimen after curing for 28 days, and the bonding strength of the material was tested by a tensile testing machine and a special tensile fixture after curing for another 14 days. The test results are shown in Table 1.

[0064] Table 1

[0065] Serial number 3d compressive strength / MPa 28d compressive strength / MPa Adhesion force / MPa Consistency / mm Example 1 25.67 43.35 1.72 80 Example 2 27.43 43.91 1.91 82 Example 3 29.58 49.16 1.99 86 Comparative Example 1 15.17 33.75 1.21 100 Comparative Example 2 24.95 36.25 1.23 102

[0066] It can be seen from the results in Table 1 that the solid waste-based shotcrete material prepared by the present invention has a 3d compressive strength greater than 20 MPa and a 28d compressive strength greater than 42.5 MPa compared with "GB 175-2023 General Portland Cement", which meets the strength of 42.5 grade Portland cement and has excellent early strength performance. When used in actual construction, it is beneficial to shorten the construction period and save costs.

[0067] Both the bonding strength and consistency meet the requirements of "JGJ / T 283-2011 Technical Code for Concrete Base Spraying Treatment" (bonding strength ≥ 0.4MPa, consistency should be 80-100mm).

[0068] The 3d compressive strength and 28d compressive strength of the solid waste-based spraying materials of Comparative Examples 1 and 2 are lower than those of the embodiments of the present application, and do not reach the 42.5 grade silicate cement strength. In addition, although the bonding force meets the requirements of "JGJ / T 283-2011 Technical Specification for Spraying Treatment of Concrete Base", the consistency fails to reach an appropriate level.

[0069] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.

Claims

1. A solid waste-based spraying material, characterized in that: It comprises 70 to 100 parts by weight of active powder and 5 to 20 parts by weight of activator; wherein the active powder is selected from at least two of coal gangue, fly ash, red mud, mineral powder, silica fume and steel slag; and the solid waste-based spraying material does not contain cement.

2. The solid waste-based shotcrete material according to claim 1, characterized in that: It also includes aggregate and water; wherein the mass of the aggregate is 50 to 400 parts by weight; and the mass of the water is 20 to 55 parts by weight.

3. The solid waste-based shotcrete material according to claim 2, characterized in that: The active powder comprises the following components: 0-30 parts by weight of coal gangue, 0-30 parts by weight of fly ash, 0-20 parts by weight of red mud, 0-50 parts by weight of mineral powder, 0-20 parts by weight of silica fume and 0-50 parts by weight of steel slag.

4. The solid waste-based shotcrete material according to claim 3, characterized in that: The active powder comprises the following components: 2 to 15 parts by weight of coal gangue, 2 to 20 parts by weight of fly ash, 5 to 20 parts by weight of red mud, 10 to 50 parts by weight of mineral powder and 10 to 50 parts by weight of steel slag.

5. The solid waste-based shotcrete material according to claim 2, characterized in that: The activator is selected from one or more of silicates, aluminates, phosphates, sulfates, carbonates, and caustic alkalis.

6. The solid waste-based shotcrete material according to claim 2, characterized in that: The aggregate is selected from one or more of tailings sand, river sand, river sand and machine-made sand.

7. The solid waste-based shotcrete material according to claim 6, characterized in that: The particle size of the aggregate is ≤4.75mm.

8. The solid waste-based spraying material according to any one of claims 2 to 7, characterized in that: The solid waste-based shotcrete material has a 3d compressive strength of >20 MPa; a 28d compressive strength of >42.5 MPa; an adhesive force of >1.3 MPa; and a consistency of 80 to 100 mm.

9. A method for preparing a solid waste-based spraying material according to any one of claims 2 to 8, characterized in that: The steps include: (1) mixing the active powder and the activator in proportion to obtain a dry mixed solid waste-based spraying material; (2) The dry mixed solid waste-based shotcrete material, aggregate and water are mixed and stirred in a ratio of 1:0.5-6:0.2-0.8 to obtain the solid waste-based shotcrete material.

10. Use of the solid waste-based shotcrete material according to any one of claims 1 to 8 and / or the solid waste-based shotcrete material obtained by the preparation method according to claim 9 in tunnel and slope protection.

Citation Information

Cited By

  • All-solid waste gel tough composite material and preparation method thereof

    CN121159218A

  • Method for synergistically preparing high-performance dry-mixed mortar from multi-source solid waste oriented by crystal structure

    CN122380721A