Self-compacting concrete composition, self-compacting concrete, and preparation method and application thereof

By combining modified gangue aggregate with silicate cement, fly ash and premature strength agent, self-condensed concrete with high strength and low water absorption is prepared, which solves the high cost of self-condensed concrete and insufficient utilization of coal gangue waste. The problem of environmental protection and resource conservation has achieved the effect of environmental protection and resource conservation.

CN119080457APending Publication Date: 2024-12-06SHENHUA BAOTOU ENERGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411202945.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing self-finished concrete is costly and cannot effectively utilize coal gangue waste, resulting in environmental pollution and waste of resources.

Method used

Using gangue aggregate modified with viscosity modified materials, combined with silicate cement, fly ash and premature strength agent, a high-strength, low-water absorption self-solid concrete is prepared to replace natural gravel. Reduce the water absorption and crushing value of coal gangue, and improve its reaction capacity with other raw materials through modification treatment.

Benefits of technology

It significantly improves the strength and water absorption rate of concrete, reduces the pollution of coal gangue to the environment, realizes efficient use of waste and resource conservation, and solves the problem of coal gangue stacking pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005018250650000111
    Figure BDA0005018250650000111
  • Figure BDA0005018250650000121
    Figure BDA0005018250650000121
Patent Text Reader

Abstract

The invention provides a self-compacting concrete composition, self-compacting concrete, and a preparation method and application thereof. The self-compacting concrete composition is prepared from 300 to 400 parts of Portland cement, 150 to 200 parts of water, 10 to 15 parts of a water reducing agent, 150 to 200 parts of fly ash, 300 to 680 parts of coal gangue aggregate and 15 to 25 parts of an early strength agent, wherein the coal gangue aggregate is coal gangue modified by a viscosity modification material; the viscosity modified material comprises kaolin, coal gangue chippings and biomass fly ash, and the mass ratio of the kaolin to the coal gangue chippings to the biomass fly ash is (0.5-1.5): (0.5-1.5): (1.5-2.5). The coal gangue aggregate formed by modifying the coal gangue through the viscosity modification material can reduce the water absorption and the crushing value of the coal gangue, can promote the coal gangue to react with other raw materials better, can replace broken stones, has economic benefits, and can solve the problem of environmental pollution of the coal gangue.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of mine concrete, and in particular to a self-compacting concrete composition, self-compacting concrete, and a preparation method and application thereof. Background Art

[0002] Self-compacting concrete refers to concrete that can flow and compact under its own gravity, can completely fill the formwork even in the presence of dense steel bars, and has good homogeneity and does not require additional vibration. Self-compacting concrete also has the following advantages: it can ensure good compaction of concrete, improve production efficiency, improve working environment and safety, increase the freedom of structural design, improve the surface quality of concrete, and reduce the wear of concrete on mixers, etc. However, the durability of self-compacting concrete after hardening is very limited, especially in cold climates. At present, the self-compacting concrete in related technologies still has the problem that the 28d compressive strength is difficult to meet the expected design standards.

[0003] At present, there are more and more research reports on the use of various types of coal gangue in concrete. For example, the patent with application number 201910432285.9 discloses a method of preparing self-compacting concrete using coal gangue. The components include coal gangue, river sand, fly ash, natural aggregate, cement, water reducer and water. The obtained self-compacting concrete has good anti-segregation and self-filling properties, but the amount of coal gangue aggregate added is small and the utilization rate is not high. The patent with application number CN202211311908.5 discloses a C60 high-performance self-compacting concrete suitable for arch structures, which is composed of cement, fly ash, mineral powder, fine aggregate, coarse aggregate, steel fiber, dispersant, water reducer, and water. The concrete obtained has high strength performance, but the waste is rarely used, and the waste utilization cannot be effectively solved. Although the above two patents use solid waste to prepare self-compacting concrete, they can only solve the accumulation problem of some gangue mountains, and the amount of waste used is limited, and other gangue utilization problems cannot be solved. In view of this, the development of a self-compacting concrete with high utilization rate using gangue waste as the main raw material can effectively solve the problem of stacking of gangue waste in my country.

[0004] my country is the world's largest coal producer and user, so its coal gangue emissions are also among the highest in the world. Coal gangue is a black-gray rock that is harder than coal and has a low carbon content and accompanies coal seams during the coal-forming process. Coal gangue has a certain volcanic ash activity due to the presence of amorphous SiO2 and Al2O3, and is usually added to concrete as a coarse aggregate.

[0005] As the underground working face advances, the floor unloads and bulges. Due to the humid underground environment, the underground floor road softens when it encounters water, and the road bearing capacity drops sharply, which cannot meet the needs of equipment transportation and vehicle traffic on the working face. When the working face begins to arrange and install large-scale mining equipment, the frequency of underground equipment transportation and vehicle driving continues to increase. Therefore, this requires the concrete floor to have a certain strength to meet the needs of vehicle traffic.

[0006] Using solid waste to replace crushed stone to prepare concrete is an effective way to alleviate environmental and resource pressures. my country is a major coal consumer, but the solid waste gangue generated during coal mining and production cannot be reasonably utilized. Therefore, how to solve the serious environmental pollution caused by the large accumulation of gangue is also an urgent problem to be solved. Summary of the invention

[0007] The main purpose of the present invention is to provide a self-compacting concrete composition, self-compacting concrete, and a preparation method and application thereof, so as to solve the problems of high cost of self-compacting concrete and environmental pollution caused by large amount of coal gangue accumulation in the prior art.

[0008] In order to achieve the above-mentioned object, according to one aspect of the present invention, a self-compacting concrete composition is provided, which comprises, by weight, 300-400 parts of silicate cement, 150-200 parts of water, 10-15 parts of a water reducing agent, 150-200 parts of fly ash, 300-680 parts of coal gangue aggregate, and 5-25 parts of an early strength agent; the coal gangue aggregate is coal gangue modified by a viscosity modifying material; the viscosity modifying material comprises kaolin, coal gangue chips and biomass fly ash, and the mass ratio of kaolin, coal gangue chips and biomass fly ash is 0.5-1.5:0.5-1.5:1.5-2.5.

[0009] Further, according to weight parts, it includes: 330-340 parts of silicate cement, 190-200 parts of water, 10-12 parts of water reducing agent, 150-160 parts of fly ash, 325-335 parts of coal gangue aggregate, and 5-15 parts of early strength agent; preferably, according to weight parts, the self-compacting concrete composition includes: 335 parts of silicate cement, 195 parts of water, 10 parts of water reducing agent, 150 parts of fly ash, 330 parts of coal gangue aggregate, and 15 parts of early strength agent;

[0010] The particle size of coal gangue aggregate is 5-20mm, and the apparent density is 2350-2513kg / m 3 ;

[0011] Preferably, the component with a particle size of 5-10 mm in the coal gangue aggregate accounts for 40wt%-50wt%, and the component with a particle size of 10-20 mm in the coal gangue aggregate accounts for 50wt%-60wt%.

[0012] Furthermore, the content of kaolinite in the coal gangue aggregate is 30% to 45%.

[0013] The auto-ignition point of coal gangue is between 300 and 500°C.

[0014] The calorific value of coal gangue is 3300~6300kJ / kg;

[0015] The viscosity modifying material further includes a catalyst, and the catalyst includes any one or more of hydroxypropylmethylcellulose and polyacrylamide.

[0016] Furthermore, the preparation method of coal gangue aggregate comprises the following steps: step A1, crushing, screening and compounding coal gangue to obtain coal gangue coarse aggregate with a particle size of 5 to 20 mm, wherein powder dropped during the screening process is collected to obtain debris; step A2, mixing metakaolin, debris and biomass fly ash in proportion, grinding them, and mixing them with a catalyst to obtain a viscosity-modified material; step A3, mixing the coal gangue coarse aggregate and a viscosity modifier to obtain coal gangue aggregate;

[0017] Preferably, step A3 includes: step A31, mixing kaolin, debris and biomass fly ash in proportion and grinding them to obtain a first viscosity modifying material precursor; step A32, mixing polyacrylamide with water to form a polyacrylamide solution, and mixing the polyacrylamide solution with the first viscosity modifying material precursor to obtain a second viscosity modifying material precursor; step A33, mixing the second viscosity modifying material precursor with hydroxypropyl methylcellulose and a polycarboxylic acid water reducer to obtain a viscosity modifying material.

[0018] Furthermore, step A1 further comprises pre-treating the gangue raw material to obtain pre-treated gangue; the pre-treating comprises crushing, screening and washing;

[0019] Preferably, the content of needle-like particles in the pretreated coal gangue is no more than 10%, the mud content is no more than 1.0%, and the crushing value is no more than 15%;

[0020] Preferably, the content of kaolinite in the coal gangue raw material is 30%-45%.

[0021] Further, the silicate cement is PO 42.5 cement;

[0022] The fly ash is Class I fly ash, and the apparent density of fly ash is 1900~2750kg / m 3 ;

[0023] The water reducing agent is a polycarboxylic acid, and preferably, the polycarboxylic acid comprises an early-strength polycarboxylic acid and a slow-release polycarboxylic acid in a weight ratio of 4:1;

[0024] The early strength agent comprises triethanolamine and sodium sulfate in a weight ratio of 1 to 2:1.

[0025] According to another aspect of the present application, a self-compacting concrete is provided. The self-compacting concrete is prepared from any one of the above self-compacting concrete compositions.

[0026] According to another aspect of the present application, a method for preparing the above-mentioned self-compacting concrete is provided, and the preparation method includes: step B1, mixing silicate cement and fly ash to obtain a gel material; step B2, mixing the gel material with coal gangue aggregate to obtain a first mixture; step B3, dissolving a water reducer in water to obtain a water reducer solution, mixing the water reducer solution with the first mixture to obtain a second mixture; step B4, dissolving an accelerator in water to obtain an accelerator solution, mixing the accelerator solution with the second mixture to obtain a self-compacting concrete slurry; step B5, pouring and curing the self-compacting concrete slurry to obtain a self-compacting concrete.

[0027] Furthermore, in step B4, the stirring comprises: first stirring at 200-250 r / min for 1-3 min, and then stirring at 500-600 r / min for 3-5 min.

[0028] According to another aspect of the present application, there is provided an application of the self-compacting concrete described above or the self-compacting concrete prepared by any of the preparation methods described above as an underground floor.

[0029] By applying the technical solution of the present invention, the gangue aggregate formed by modifying the gangue with the viscosity modifying material can reduce the water absorption and crushing value of the gangue, promote the gangue to react better with other raw materials, and replace crushed stone, which has economic benefits, can also realize the call for green environmental protection, and solve the problem of environmental pollution. Furthermore, the gangue used in the present invention can not only replace natural crushed stone to make concrete with a strength in the range of C15-C40, but also significantly improve the strength and water absorption of concrete. The use of gangue to prepare concrete instead of natural crushed stone can not only reduce the pollution of the soil and atmospheric environment by the gangue, but also save natural non-renewable materials. At the same time, the amount of gangue used in the present invention is relatively large, which can effectively solve the problems of environmental pollution caused by the stacking of gangue in my country, as well as the recycling of waste. DETAILED DESCRIPTION

[0030] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0031] As analyzed in the background technology of this application, the prior art has the problems of high cost of self-compacting concrete and environmentally unfriendly large-scale accumulation of coal gangue. In order to solve this problem, this application provides a self-compacting concrete composition, self-compacting concrete, and a preparation method and application thereof.

[0032] According to a typical embodiment of the present application, a self-compacting concrete composition is provided, which comprises, by weight, 300-400 parts of silicate cement, 150-200 parts of water, 10-15 parts of a water reducer, 150-200 parts of fly ash, 300-680 parts of coal gangue aggregate, and 5-25 parts of an early strength agent; wherein the coal gangue aggregate is coal gangue modified by a viscosity modifying material; the viscosity modifying material comprises kaolin, coal gangue fragments and biomass fly ash, wherein the mass ratio of kaolin, coal gangue fragments and biomass fly ash is 0.5-1.5:0.5-1.5:1.5-2.5.

[0033] The gangue aggregate formed by modifying the gangue with the viscosity modifying material can reduce the water absorption and crushing value of the gangue, can promote the gangue to react better with other raw materials, can replace crushed stone, has economic benefits, and can realize the call for green environmental protection and solve the problem of environmental pollution. Further, the gangue used in the present invention can not only replace natural crushed stone to make concrete with a strength in the range of C15-C40, but also significantly improve the strength and water absorption of concrete. The use of gangue to prepare concrete instead of natural crushed stone can reduce the pollution of the soil and atmospheric environment by the gangue, and can save natural non-renewable materials. At the same time, the amount of gangue used in the present invention is relatively large, which can effectively solve the problems of environmental pollution caused by the stacking of gangue in my country, as well as waste recycling.

[0034] In some embodiments of the present application, in order to better exert the synergistic effect of each component, the self-compacting concrete composition comprises, by weight: 330-340 parts of Portland cement, 190-200 parts of water, 10-12 parts of water reducer, 150-160 parts of fly ash, 325-335 parts of coal gangue aggregate, and 5-15 parts of early strength agent. Preferably, by weight, the self-compacting concrete composition comprises: 335 parts of Portland cement, 195 parts of water, 10 parts of water reducer, 150 parts of fly ash, 330 parts of coal gangue aggregate, and 15 parts of early strength agent.

[0035] In some embodiments of the present application, the particle size of the gangue aggregate is 5-20 mm, and the apparent density is 2350-2513 kg / m 3, which helps to further improve the strength of the self-compacting concrete. In some preferred embodiments of the present application, the component with a particle size of 5-10mm in the gangue aggregate accounts for 40wt%-50wt%, and the component with a particle size of 10-20mm in the gangue aggregate accounts for 50wt%-60wt%, which can make the gangue aggregate and other combinations in the self-compacting concrete composition better play a synergistic role and further improve the strength and mechanical properties of the self-compacting concrete. More preferably, the component with a particle size of 5-10mm in the gangue aggregate accounts for 45wt%, and the component with a particle size of 10-20mm in the gangue aggregate accounts for 55wt%.

[0036] In some embodiments of the present application, the coarse and fine aggregates of coal gangue are added into a mixer with a rotation speed of 250 to 500 r / min and stirred for 2 to 5 minutes to obtain a mixed aggregate, preferably, stirred for 3 minutes.

[0037] In some embodiments of the present application, the content of kaolinite in the gangue aggregate is 30% to 55%, preferably 30% to 45%. Kaolinite is formed by aluminum silicate minerals such as feldspar and common pyroxene during the weathering process, has low hardness, plasticity, adhesion and volume expansion when wet, and the gangue aggregate with this kaolinite content can further improve the strength of the self-compacting concrete, and has good compactness, and is easy to use and maintain. Increasing the content of kaolinite in the gangue aggregate is helpful to improve the strength of the self-compacting concrete, but considering the current composition of the gangue and reducing the environmental pollution caused by the accumulation of the gangue, when the content of kaolinite in the gangue aggregate is 30% to 45%, the strength of the self-compacting concrete can be guaranteed and the use requirements can be met, especially in the application of underground floor plates, and the source is relatively wide, solving the environmental problems caused by the gangue.

[0038] In some embodiments of the present application, the auto-ignition point of the above-mentioned coal gangue is between 300 and 500° C., and the calorific value of the coal gangue is between 3300 and 6300 kJ / kg, which can enable the self-compacting concrete to achieve better results.

[0039] In some embodiments of the present application, the viscosity modifying material further comprises a catalyst, and the catalyst comprises any one or more of hydroxypropyl methylcellulose (HPMC) and polyacrylamide (PAM). Preferably, the molecular weight of polyacrylamide (PAM) is 24 million.

[0040] In some preferred embodiments of the present application, the catalyst includes a mixture of hydroxypropyl methylcellulose and polyacrylamide. The amount of the catalyst can be determined according to the amount of Portland cement in the self-compacting concrete. In some embodiments of the present application, the mass of the catalyst is 0.3% to 1% of the mass of the Portland cement in the self-compacting concrete composition. In some preferred embodiments of the present application, the amount of polyacrylamide (PAM) added is 0.3% of the mass of the Portland cement, and the amount of hydroxypropyl methylcellulose (HPMC) added is 0.1% of the mass of the Portland cement.

[0041] The above-mentioned biomass fly ash is produced after the combustion of biomass fuel, such as biomass fly ash, wherein the biomass fuel includes but is not limited to corn stalks, wood chips, and peanut shells. The biomass fly ash in the viscosity modifying material can increase the fluidity of the coal gangue aggregate.

[0042] In some typical embodiments of the present application, the above-mentioned gangue aggregate is prepared by the following steps: Step A1, crushing, screening and compounding the gangue to obtain a coarse gangue aggregate with a particle size of 5 to 20 mm, wherein the powder dropped during the screening process is collected to obtain debris; Step A2, mixing metakaolin, debris and biomass fly ash in proportion for grinding, mixing with a catalyst to obtain a viscosity-modified material; Step A3, mixing the coarse gangue aggregate and the viscosity modifier to obtain the gangue aggregate. Since the strength of concrete is not high when the amount of gangue doping is large, after it is modified, its mechanical properties can meet the strength requirements of the C15 to C40 concrete specifications, so that the added value of the gangue can be quickly converted. Crushing, screening and modifying the gangue can effectively reduce its water absorption, making the preparation of concrete environmentally friendly and efficient, saving a lot of energy, improving workability, facilitating industrial production, and producing gangue concrete with better mechanical properties. The gangue concrete can also be applied to the field of concrete component preparation technology.

[0043] In some embodiments of the present application, the above step A1 also includes pre-treating the gangue raw material to obtain pre-treated gangue, and typically, the pre-treatment includes crushing, screening, and washing. Pre-treating the gangue aggregate can reduce the water absorption and crushing value of the gangue aggregate. This pre-treatment can better promote the modification of the gangue and facilitate the reaction of the modified gangue aggregate with other raw materials.

[0044] In some embodiments of the present application, the above-mentioned coal gangue raw material is self-igniting coal gangue, which is brown-red in color, and the red color in the coal gangue comes from the oxidation of iron oxides in the coal gangue.

[0045] In some embodiments of the present application, the content of kaolinite in the gangue raw material is 30%-45%. The kaolinite in the gangue raw material has been converted into metakaolin, has high volcanic ash activity, and can be thickened.

[0046] In some embodiments of the present application, the above-mentioned pretreatment includes: placing the coal gangue into a jaw crusher with a rotation speed of 250r / min and a power of 5.5kw for crushing, and then passing through 5-10mm and 10-20mm square hole sieves and compounding them in proportion to obtain coal gangue coarse aggregate; collecting a large amount of kaolin and impurity debris fallen off during the crushing of the coal gangue, and passing them through a 5mm sieve, and after the kaolin and impurity debris with a particle size of less than 5mm are mixed with biomass fly ash in proportion, grinding them for 30min to 60min to prepare a powder viscosity modified material.

[0047] In some embodiments of the present application, the above-mentioned washing includes: washing the gangue coarse aggregate to wash out part of the coal quality and dust, and spontaneously drying the primary screened material for modification. The primary screened material is washed and dried to obtain pretreated aggregate, which can effectively reduce its water absorption, making the preparation environmentally friendly and efficient, saving a lot of energy, improving workability, facilitating industrial production, and obtaining gangue concrete with better mechanical properties.

[0048] In some preferred embodiments of the present application, the content of needle-like particles in the pretreated coal gangue is not more than 10%, the mud content is not more than 1.0%, and the crushing value is not more than 15%.

[0049] In some embodiments of the present application, the above step A3 includes: step A31, mixing metakaolin, debris and biomass fly ash in proportion and grinding them to obtain a first viscosity modifying material precursor; step A32, mixing polyacrylamide with water to form a polyacrylamide solution, mixing the polyacrylamide solution with the first viscosity modifying material precursor to obtain a second viscosity modifying material precursor; step A33, mixing the second viscosity modifying material precursor with hydroxypropyl methylcellulose and polycarboxylate water reducer to obtain a viscosity modifying material. Preferably, the polycarboxylate water reducer is 0.3% to 0.8% of the mass of the second viscosity modifying material precursor, and preferably, the polycarboxylate water reducer is 0.5% of the mass of the second viscosity modifying material precursor.

[0050] The silicate cement in the self-compacting concrete composition can be selected from the prior art, and the present application has no special requirements for this. For example, the silicate cement can be PO 42.5 cement.

[0051] In some embodiments of the present application, in order to further improve the strength and density of the self-compacting concrete, the fly ash is Class I fly ash, and the apparent density of the fly ash is 1900-2750 kg / m 3, which can inhibit shrinkage cracking of concrete pouring and is beneficial to the stability of the long-term strength of self-compacting concrete.

[0052] In some embodiments of the present application, the fly ash in the composition is spherical particle industrial waste produced by thermal power plants, with a smooth surface and a dense texture. The ball effect can reduce the interaction between particles, reduce water consumption and improve the fluidity of concrete, reduce the heat release of cement hydration, replace part of the cement to reduce carbon dioxide emissions, and avoid cracking of concrete during curing due to excessive heating.

[0053] The water reducer can be selected from the prior art, such as polycarboxylic acid. In some embodiments of the present application, in order to further improve the strength of the self-compacting concrete and facilitate construction, the polycarboxylic acid includes an early-strength polycarboxylic acid and a slow-release polycarboxylic acid. Preferably, the polycarboxylic acid includes an early-strength polycarboxylic acid and a slow-release polycarboxylic acid in a weight ratio of 2 to 6:1. More preferably, the polycarboxylic acid includes an early-strength polycarboxylic acid and a slow-release polycarboxylic acid in a weight ratio of 4:1.

[0054] The above-mentioned early strength agent can be selected from the prior art. In some preferred embodiments of the present application, the early strength agent includes triethanolamine and sodium sulfate in a weight ratio of 1 to 2:1, which has a more significant early strengthening effect on the self-compacting concrete with high coal gangue content in the present application.

[0055] According to another typical embodiment of the present application, a self-compacting concrete is provided. The self-compacting concrete is prepared from any one of the above-mentioned self-compacting concrete compositions.

[0056] The self-compacting concrete formed by the self-compacting concrete composition has high strength and high toughness, good overall performance, can meet the use requirements of concrete, and achieves the purpose of waste recycling while having excellent comprehensive performance. Among them, the gangue aggregate formed by modifying the gangue with the viscosity modifying material can reduce the water absorption and crushing value of the gangue, can promote the gangue to react better with other raw materials, can replace crushed stone, has economic benefits, and can realize the call for green environmental protection and solve environmental pollution problems. Further, the present invention uses gangue to not only replace natural crushed stone to make concrete with a strength in the range of C15-C40, but also significantly improve the strength and water absorption of concrete. Using gangue to prepare concrete to replace natural crushed stone can not only reduce the pollution of the soil and atmospheric environment by the gangue, but also save natural non-renewable materials. At the same time, the amount of gangue used in the present invention is large, which can effectively solve the problems of environmental pollution caused by the stacking of gangue in my country and waste recycling.

[0057] According to another typical embodiment of the present application, a method for preparing the above-mentioned self-compacting concrete is provided, and the preparation method includes: step B1, mixing silicate cement and fly ash to obtain a gel material; step B2, mixing the gel material with coal gangue aggregate to obtain a first mixture; step B3, dissolving a water reducer in water to obtain a water reducer solution, mixing the water reducer solution with the first mixture to obtain a second mixture; step B4, dissolving an accelerator in water to obtain an accelerator solution, mixing the accelerator solution with the second mixture to obtain a self-compacting concrete slurry; step B5, pouring and curing the self-compacting concrete slurry to obtain a self-compacting concrete.

[0058] The self-compacting concrete formed by the above-mentioned preparation method uses coal gangue instead of natural crushed stone to make concrete with a strength in the range of C15-C40, which can significantly improve the strength and water absorption of concrete. Using coal gangue to prepare concrete instead of natural crushed stone can not only reduce the pollution of coal gangue to the soil and atmospheric environment, but also save natural non-renewable materials. At the same time, the amount of coal gangue used in the present invention is relatively large, which can effectively solve the problems of environmental pollution caused by coal gangue stacking and waste recycling in my country.

[0059] In some preferred embodiments of the present application, in step B4, stirring includes: first stirring at 200-250r / min for 1-3min, and then stirring at 500-600r / min for 3-5min, which can make the rubber have suitable fluidity, facilitate pouring, and help improve the strength of concrete.

[0060] The self-compacting concrete slurry of the present application can be poured and cured according to the existing method, and there is no special requirement for this. Further, the curing method of the gangue self-compacting concrete is standard curing.

[0061] In some embodiments of the present application, the preparation method of the above-mentioned self-compacting concrete slurry includes the following steps: (1) adding the graded crushed and modified coarse and fine aggregates of coal gangue to a mixer at 250-500 r / min and stirring for 180 seconds to obtain a mixed aggregate. (2) weighing the cement and fly ash in the cementitious material according to the designed mix ratio, adding them and stirring and mixing, stirring for 100 seconds to obtain a cementitious material. (3) putting the mixed aggregate and the cementitious material into a mixer and stirring at a uniform speed for 2 minutes. (4) weighing the early strength polycarboxylic acid and the slow-release polycarboxylic acid in a weight ratio of 4:1 of the water reducer, stirring and dissolving them with the mixing water used, adding them to the mixer, and slowly and evenly stirring for 3 minutes. (5) Then weigh triethanolamine and sodium sulfate in a weight ratio of 2:1 as an early strength agent and stir and dissolve them with the mixing water used. Stir slowly and evenly for 2 minutes. Slowly pour the evenly stirred mixed solution into a mixer. Stir at 200-250 r / min for 1-3 minutes and then stir at 500-600 r / min for 3-5 minutes to obtain a coal gangue self-compacting concrete slurry, which has good fluidity and high strength after curing.

[0062] According to another typical embodiment of the present application, there is provided an application of the self-compacting concrete or the self-compacting concrete prepared by any of the preparation methods as an underground floor. The use of the self-compacting concrete as an underground floor not only has a large bearing capacity and is adaptable to the humid environment underground, but also uses coal gangue instead of natural crushed stone, which can reduce the pollution of coal gangue to the soil and atmospheric environment, and can also use local materials to save natural non-renewable materials. At the same time, the amount of coal gangue used in the present invention is relatively large, which can effectively solve the problems of coal gangue stacking polluting the environment and waste recycling in my country.

[0063] The beneficial effects that can be achieved by the present application will be further illustrated below in combination with embodiments and comparative examples.

[0064] Example 1

[0065] The present embodiment provides a self-compacting concrete composition prepared by using coal gangue, and the specific proportion is: 330kg coal gangue aggregate, 195kg water, 390kg Portland cement, 6.25kg early strength polycarboxylic acid (yellow-brown liquid JS05240520017), 3.75kg slow-release polycarboxylic acid (JS06240520016, light yellow liquid form, implemented in accordance with the standard: GB / T 8076-2008 "Concrete Admixtures"), 6.67kg triethanolamine, 3.33kg sodium sulfate, 150kg fly ash (Grade I fly ash, loss on ignition ≤3.0%, 45μm sieve residue ≤12%, water demand ratio ≤95%, moisture content ≤1.0%). Among them, the components with a particle size of 5-10 mm account for 45% of the coal gangue aggregate, and the components with a particle size of 10-20 mm account for 55% of the coal gangue aggregate.

[0066] The preparation method of coal gangue aggregate is as follows:

[0067] Manual sampling: After careful manual screening at the gangue dump, gangue with the characteristics of spontaneous combustion gangue (brown-red gangue) was selected for recycling and transported to the laboratory. The kaolinite content in the selected gangue was 40wt%.

[0068] Crushing: Put the coal gangue with particle size ≥20mm into a jaw crusher with a speed of 250r / min and a power of 5.5kw for crushing.

[0069] Screening: Coal gangue is screened as aggregate: after screening the coal gangue using 5-10mm and 10-20mm square hole screens, remove the coal gangue with a particle size of less than 5mm to obtain primary screening materials. The particle size of the primary screening materials should be ≥5mm and ≤20mm. The materials are graded according to the particle size to combine 5-20mm continuous graded coal gangue coarse aggregates, of which the coal gangue component with a particle size of 5-10mm accounts for 45%, and the component with a particle size of 10-20mm accounts for 55%. By collecting the powder that falls off during the screening process of coal gangue, impurity debris is obtained.

[0070] Washing: Wash out some of the coal and dust, and dry the primary screened material naturally.

[0071] Modification: ① Pass the impurity debris through a 5mm sieve, mix the metakaolin and impurity debris in a ratio of 1:1, and add biomass fly ash equal to the total mass of the two, which is the combustion product of biomass such as corn stalks, sawdust, and peanut shells. Put kaolin, debris, biomass fly ash and other materials into an electric mixer, dry mix at a speed of 150r / min for three minutes, and grind after mixing evenly;

[0072] ②Put polyacrylamide (PAM) in a beaker and mix it with water. Mix and stir at 50r / min for 10 minutes to completely dissolve PAM. The amount of polyacrylamide used is 0.3% of the weight of silicate cement.

[0073] ③ Add the mixed emulsion in step ② to the mixture in step 1, and mix and stir at 150r / min for 1min;

[0074] ④ Then add hydroxypropyl methylcellulose (HPMC) and polycarboxylate water reducer to the mixture obtained in step ③, mix and stir at a speed of 300 r / min for 3 minutes to obtain a viscosity-modified material, wherein the amount of hydroxypropyl methylcellulose (HPMC) is 0.1% of the mass of silicate cement, and the amount of polycarboxylate water reducer is 0.5% of the total mass of the above-mentioned viscosity-modified material.

[0075] ⑤ Mix the viscosity-modified material with the washed coal gangue, stir manually for 1 minute, and obtain coal gangue aggregate.

[0076] The slurry preparation method of self-compacting concrete is as follows:

[0077] (1) Add the graded crushed and modified coal gangue coarse and fine aggregates into a mixer at 350 r / min and stir for 180 seconds to obtain mixed aggregates.

[0078] (2) The cement and fly ash in the cementitious material are weighed according to the designed mix ratio, added and stirred, and stirred for 100 seconds to obtain the cementitious material.

[0079] (3) Place the mixed aggregate and cementitious material into a mixer and stir at a constant speed for 2 minutes.

[0080] (4) The water reducing agent (early strength polycarboxylic acid and slow-release polycarboxylic acid) is stirred and dissolved with the mixing water, added into the mixer, and stirred slowly and evenly for 3 minutes.

[0081] (5) Then weigh the early strength agent (triethanolamine and sodium sulfate) and stir and dissolve it with the mixing water used, stir slowly and evenly for 2 minutes, slowly pour the evenly stirred mixed solution into the mixer, stir slowly for 3 minutes, and stir quickly for 5 minutes to obtain the coal gangue self-compacting concrete slurry.

[0082] Example 2

[0083] The present embodiment provides a self-compacting concrete composition prepared by using coal gangue, and the specific proportion is: 330kg coal gangue aggregate, 195kg water, 355kg Portland cement (PO 42.5), 6.25kg early strength polycarboxylic acid (same as in Example 1), 3.75kg slow-release polycarboxylic acid (same as in Example 1), 6.67kg triethanolamine, 3.33kg sodium sulfate, 150kg fly ash (grade I fly ash, loss on ignition ≤3.0%, 45μm sieve residue ≤12%, water demand ratio ≤95%, moisture content ≤1.0%).

[0084] The preparation method of the coal gangue aggregate and the self-compacting concrete slurry in this embodiment is the same as that in Example 1.

[0085] Example 3

[0086] The present embodiment provides a self-compacting concrete composition prepared by using coal gangue, and the specific proportion is: 330kg coal gangue aggregate, 195kg water, 325kg Portland cement, 6.25kg early strength polycarboxylic acid (same as Example 1), 3.75kg slow-release polycarboxylic acid (same as Example 1), 6.67kg triethanolamine, 3.33kg sodium sulfate, 150kg fly ash (grade I fly ash, loss on ignition ≤3.0%, 45μm sieve residue ≤12%, water demand ratio ≤95%, moisture content ≤1.0%).

[0087] Example 4

[0088] The difference from Example 1 is that the components in the self-compacting concrete composition are directly mixed and stirred for 20 minutes until they are uniform, thereby obtaining a self-compacting concrete slurry.

[0089] Example 5

[0090] The difference from Example 1 is that, in the gangue coarse aggregate, the gangue component with a particle size of 5-10 mm accounts for 30%, and the component with a particle size of 10-20 mm accounts for 70%.

[0091] Example 6

[0092] The difference from Example 1 is that, in the gangue coarse aggregate, the gangue component with a particle size of 5-10 mm accounts for 60%, and the component with a particle size of 5-10 mm accounts for 40%.

[0093] Example 7

[0094] The difference from Example 1 is that when sampling during the process of preparing the coal gangue aggregate, the content of kaolinite in the selected coal gangue is 20wt%.

[0095] Example 8

[0096] The difference from Example 1 is that when sampling during the process of preparing the coal gangue aggregate, the content of kaolinite in the selected coal gangue is 55wt%.

[0097] Example 9

[0098] The difference from Example 1 is that the specific ratio of the self-compacting concrete composition is: 400 kg coal gangue aggregate, 250 kg water, 500 kg Portland cement, 6.25 kg early strength polycarboxylic acid, 3.75 kg sustained release polycarboxylic acid, 6.67 kg triethanolamine, 3.33 kg sodium sulfate, 150 kg fly ash (Grade I fly ash, loss on ignition ≤3.0%, 45 μm sieve residue ≤12%, water demand ratio ≤95%, moisture content ≤1.0%).

[0099] Example 10

[0100] The difference from Example 1 is that the specific proportion of the self-compacting concrete composition is: 600kg aggregate coal gangue, 200kg water, 385kg Portland cement, 6.25kg early strength polycarboxylic acid (same as Example 1), 3.75kg slow-release polycarboxylic acid (same as Example 1), 6.67kg triethanolamine, 3.33kg sodium sulfate, 150kg fly ash (grade I fly ash, loss on ignition ≤3.0%, 45μm sieve residue ≤12%, water demand ratio ≤95%, moisture content ≤1.0%).

[0101] Comparative Example 1

[0102] The difference from Example 1 is that the gangue aggregate is replaced by gangue with an average particle size of 10 mm. According to the same steps (2) to (6) as in Example 1, a self-compacting concrete slurry is prepared.

[0103] The self-compacting concrete slurries prepared in the above examples and comparative examples were poured and cured for 28 days to obtain self-compacting concrete. The compressive strength, tensile strength and slump of the concrete prepared with the slurries of each example and comparative example were tested, and the test results are shown in Table 1 below.

[0104] Among them, the implementation steps of the compression test are:

[0105] 1 When the specimen reaches the test age, it should be taken out from the curing room and its size and shape should be checked for damage. The specimen should be tested as soon as possible after being taken out.

[0106] 2 Before placing the specimen on the testing machine, the surface of the specimen and the upper and lower pressure plates should be wiped clean.

[0107] 3 The side of the specimen when it is formed shall be the pressure-bearing surface. The specimen shall be placed on the lower pressure plate or pad of the testing machine, and the center of the specimen shall be aligned with the center of the lower pressure plate of the testing machine.

[0108] 4 Start the testing machine. The surface of the test piece should be in even contact with the upper and lower pressure plates or steel pads.

[0109] 5 During the test, the load should be applied continuously and evenly, and the loading speed should be 0.3MPa / s~1.0MPa / s. When the compressive strength of the cube is less than 30MPa, the loading speed should be 0.3MPa / s~0.5MPa / s; when the compressive strength of the cube is 30MPa~60MPa, the loading speed should be 0.5MPa / s~0.8MPa / s; when the compressive strength of the cube is not less than 60MPa, the loading speed should be 0.8MPa / s~1.0MPa / s.

[0110] 6 When manually controlling the loading speed of the press, when the specimen approaches failure and begins to deform rapidly, the throttle adjustment of the testing machine should be stopped until failure, and the failure load should be recorded.

[0111] Based on the standard: GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete".

[0112] Among them, the test steps of slump are:

[0113] (1) Place a dry base plate without obvious moisture on a solid horizontal surface, check whether the inner wall of the slump cone is dry, and place the slump cone in the center of the base plate, and step on the pedals on both sides of the slump cone to keep it in a fixed position;

[0114] (2) The height of the slump cone is 300 mm. In order to obtain better test results, the slump cone is loaded three times, and the height of each slurry is 100 mm. Each time the filling material is loaded, the tamping rod is used to tamp 30 times evenly from the center to the surrounding area;

[0115] (3) When tamping the first layer, the tamping rod should penetrate the entire first layer. When tamping the second and third layers, the tamping rod should penetrate the current layer and reach the surface of the next layer.

[0116] (4) During the tamping process, the filling material height of the third layer should be higher than 300mm. If the height of the mixed slurry is lower than the barrel mouth, it should be added at any time;

[0117] (5) After completing the third layer of tamping, remove the loading funnel, scrape off the excess slurry above the slump tube, and smooth it along the tube mouth;

[0118] (6) Hold the handles on both sides of the slump cone and slowly lift the slump cone. The sample will slowly collapse. Wait until the slump cone is completely removed and the slurry stops collapsing or wait for 30 seconds. Use a steel ruler to measure the height of the slurry and calculate the height difference between the slurry and the slump cone. This height difference is the slump value.

[0119] Table 1

[0120]

[0121]

[0122] The compressive strength is an important indicator to measure whether the concrete meets the standard. The concrete prepared by the mix ratio selected in Example 2 has a 28d compressive strength of 41.3 MPa and a tensile strength of 3.33 MPa, and the strength meets the basic requirements.

[0123] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects: the gangue aggregate formed by modifying the gangue with the viscosity modifying material can reduce the water absorption and crushing value of the gangue, can promote the gangue to react better with other raw materials, can replace crushed stone, has economic benefits, and can realize the call for green environmental protection and solve environmental pollution problems. Further, the present invention uses gangue to not only replace natural crushed stone to make concrete with a strength in the range of C15-C40, but also significantly improve the strength and water absorption of concrete. Using gangue to prepare concrete to replace natural crushed stone can not only reduce the pollution of the soil and atmospheric environment by the gangue, but also save natural non-renewable materials. At the same time, the amount of gangue used in the present invention is relatively large, which can effectively solve the problems of coal gangue stacking pollution in my country and waste recycling.

[0124] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A self-compacting concrete composition, characterized in that According to weight, it includes: 300-400 parts of silicate cement, 150-200 parts of water, 10-15 parts of water reducing agent, 150-200 parts of fly ash, 300-680 parts of coal gangue aggregate, and 5-25 parts of early strength agent; The gangue aggregate is gangue modified by a viscosity modifying material; the viscosity modifying material comprises kaolin, gangue debris and biomass fly ash, and the mass ratio of kaolin, gangue debris and biomass fly ash is 0.5-1.5:0.5-1.5:1.5-2.

5.

2. The self-compacting concrete composition according to claim 1, characterized in that According to weight parts, it includes: 330-340 parts of silicate cement, 190-200 parts of water, 10-12 parts of water reducing agent, 150-160 parts of fly ash, 325-335 parts of coal gangue aggregate, and 5-15 parts of early strength agent; preferably, according to weight parts, the self-compacting concrete composition includes: 335 parts of silicate cement, 195 parts of water, 10 parts of water reducing agent, 150 parts of fly ash, 330 parts of coal gangue aggregate, and 15 parts of early strength agent; The particle size of the coal gangue aggregate is 5-20 mm, and the apparent density is 2350-2513 kg / m 3 ; Preferably, the component with a particle size of 5-10 mm in the coal gangue aggregate accounts for 40wt%-50wt%, and the component with a particle size of 10-20 mm in the coal gangue aggregate accounts for 50wt%-60wt%.

3. The self-compacting concrete composition according to claim 1, characterized in that The content of kaolinite in the coal gangue aggregate is 30% to 45%. The auto-ignition point of the coal gangue is between 300 and 500°C. The calorific value of the coal gangue is 3300-6300 kJ / kg; The viscosity modifying material further comprises a catalyst, and the catalyst comprises any one or more of hydroxypropyl methylcellulose and polyacrylamide.

4. The self-compacting concrete composition according to claim 3, characterized in that The preparation method of the coal gangue aggregate comprises the following steps: Step A1, crushing, sieving, and compounding the coal gangue to obtain a coarse aggregate of coal gangue with a particle size of 5 to 20 mm, wherein the powder dropped during the sieving process is collected to obtain debris; Step A2, mixing the metakaolin, the debris and the biomass fly ash in proportion, grinding them, and mixing them with a catalyst to obtain a viscosity-modified material; Step A3, mixing the gangue coarse aggregate and the viscosity modifier to obtain the gangue aggregate; Preferably, step A3 comprises: Step A31, mixing the metakaolin, the debris and the biomass fly ash in proportion and grinding them to obtain a first viscosity-modifying material precursor; Step A32, mixing polyacrylamide with water to form a polyacrylamide solution, and mixing the polyacrylamide solution with the first viscosity modifying material precursor to obtain a second viscosity modifying material precursor; Step A33, mixing the second viscosity modifying material precursor with hydroxypropyl methylcellulose and polycarboxylic acid water reducer to obtain the viscosity modifying material.

5. The self-compacting concrete composition according to claim 4, characterized in that Step A1 also includes pre-treating the gangue raw material to obtain pre-treated gangue; the pre-treatment includes crushing, screening, and washing; Preferably, the content of needle-like particles in the pretreated coal gangue is no more than 10%, the mud content is no more than 1.0%, and the crushing value is no more than 15%; Preferably, the content of kaolinite in the coal gangue raw material is 30%-45%.

6. The self-compacting concrete composition according to any one of claims 1 to 3, characterized in that The silicate cement is PO 42.5 cement; The fly ash is Class I fly ash, and the apparent density of the fly ash is 1900-2750 kg / m 3 ; The water reducing agent is a polycarboxylic acid, and preferably, the polycarboxylic acid comprises an early-strength polycarboxylic acid and a slow-release polycarboxylic acid in a weight ratio of 4:1; The early strength agent comprises triethanolamine and sodium sulfate in a weight ratio of 1 to 2:

1.

7. A self-compacting concrete, characterized in that: Prepared from the self-compacting concrete composition according to any one of claims 1 to 6.

8. A method for preparing the self-compacting concrete according to claim 7, characterized in that: include: Step B1, mixing silicate cement and fly ash to obtain a gel material; Step B2, mixing the gel material with coal gangue aggregate to obtain a first mixed material; Step B3, dissolving a water reducer in water to obtain a water reducer solution, and mixing the water reducer solution with the first mixed material to obtain a second mixed material; Step B4, dissolving the early strength agent in water to obtain an early strength agent solution, and mixing the early strength agent solution with the second mixed material to obtain a self-compacting concrete slurry; Step B5, pouring and curing the self-compacting concrete slurry to obtain self-compacting concrete.

9. The preparation method according to claim 8, characterized in that: In the step B4, the stirring comprises: first stirring at 200-250 r / min for 1-3 min, and then stirring at 500-600 r / min for 3-5 min.

10. Use of the self-compacting concrete according to claim 7 or the self-compacting concrete prepared by the preparation method of claim 8 or 9 as an underground floor.

Citation Information

Patent Citations

  • Mining FRP grill-gangue-self-compacting concrete regenerated roof and construction method thereof

    CN110118089A

  • C60 high-performance self-compacting concrete suitable for arched structure and preparation method thereof

    CN115536340A