Nanometer thermal insulation board and preparation method and application thereof

The nano-thermal insulation board prepared by dry method solves the problems of reduced insulation performance and high cost of electric vehicle batteries at high temperatures, achieves stable insulation performance and low cost, and improves the safety and escape time of electric vehicle batteries. .

CN119080472APending Publication Date: 2024-12-06ZHENGZHOU HOLLOWLITE MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411195775.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing battery insulation film has deteriorated performance at high temperatures, high cost, and complex preparation process, resulting in insufficient safety of electric vehicle batteries and an increase in the risk of explosion.

Method used

The nano-thermal insulation board prepared by dry method is mainly composed of hollow glass microspheres, thermal insulation powder, sunscreen agent, fiber and hydrophobic agent. It is made by dry mixing, molding and hydrophobic treatment, and has good thermal insulation properties and Compression performance, suitable for high temperature environments of 350-650℃.

Benefits of technology

It achieves low-cost and stable thermal insulation performance, improves the safety of electric vehicle batteries, extends escape time, reduces explosive destructiveness, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention provides a nano heat insulation plate as well as a preparation method and application thereof. The nanometer heat insulation plate is mainly prepared from the following raw materials in parts by mass through dry mixing, compression molding and hydrophobic treatment: 10-30 parts of hollow glass microspheres, 50-70 parts of heat insulation powder, 5-20 parts of an opacifying agent, 2-10 parts of fibers and a water repellent agent, and the dosage of the water repellent agent is 30-180 kg / m < 3 > according to the volume of the nanometer heat insulation plate. The nanometer heat insulation plate is prepared by adopting a dry method, has the characteristics of good heat insulation performance, uniform texture, stable compression performance, long-term service with the highest temperature range of 350-650 DEG C, low production cost and the like, and is suitable for a heat insulation film for a battery cell of a common electric automobile. Therefore, the invention also provides an application of the nano heat insulation plate in preparation of a battery, in particular an application of the nano heat insulation plate in preparation of a heat insulation film of a battery cell of the battery for an electric vehicle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a nano heat insulation board and a preparation method and application thereof. Background Art

[0002] With the development of new energy vehicles, electric vehicles are gradually entering the market, and the demand for longer driving range is becoming increasingly prominent. To solve this problem, the battery energy density is required to be higher and higher. As the battery energy density gradually increases, the battery cycle expansion rate gradually increases, which leads to a gradual decrease in the safety of the battery itself. After forming a module, the expansion force between the cells increases, the probability of thermal runaway of the battery increases, and the probability of explosion affecting the life safety of personnel also increases.

[0003] In order to reduce the risk of thermal runaway between batteries, thermal insulation films are usually installed between batteries. It is usually hoped that when a battery cell experiences thermal runaway and the temperature rises sharply or even catches fire, it will not cause chain runaway of the adjacent battery cell, and it will give people more than 15 minutes to escape, reducing the destructive power of electric vehicle explosions without causing fundamental damage to the vehicle body. Battery thermal insulation films must withstand a certain amount of pressure during actual use. This pressure is the pressure during the actual thermal failure of the battery. The product needs to form a certain amount of compression under this pressure to prevent product damage due to unstable product compression, thereby directing the heat of the explosion to other batteries.

[0004] Silica aerogel is a new type of lightweight and efficient thermal insulation material with special properties such as low density, high porosity, and low thermal conductivity. However, it is brittle and has low strength. When the temperature is high, the aerogel will lose its porous structure, resulting in a decrease in thermal insulation. In addition, the cost of silica aerogel is relatively high. Moreover, the better the high temperature resistance of the thermal insulation material, the more expensive its production cost and sales price are.

[0005] To this end, Chinese patent application CN 116638831 A is a highly efficient heat-insulating flame-retardant material between monomer cells, including a core layer, wherein the core layer is a heat-insulating fiber felt composited with silica aerogel and hollow ceramic fibers, and the core layer is coated with a buffer layer on both sides, wherein the buffer layer is a foamed polyurethane composite modified by modified graphene and modified hollow glass microspheres, and the modified hollow glass microspheres are obtained by grafting diphenylmethane diisocyanate after coating the surface of the glass microspheres with a nano-titanium dioxide film. Although the above patent application has uniform heat-insulating performance, it mainly realizes the heat-insulating layer of compression control by means of a buffer layer through a ceramic aerogel composite felt, and the hollow ceramic fiber is expensive, and the market cannot accept the product price when it is composited with an aerogel felt. The heat-insulating core material is wrapped with a buffer layer, which will form a thermal bridge, resulting in heat conduction, and the wrapping process is complicated, resulting in high cost, and the foamed polyurethane is flammable. Even if a flame retardant is added, the structure will be destroyed at high temperature, and the heat will be transferred to other cells. In addition, the preparation of the core layer in the above-mentioned high-efficiency heat-insulating flame-retardant material is to use organic silicon to hydrolyze and polymerize under the action of a catalyst, and then compound it with ceramic fiber felt to form a ceramic fiber aerogel felt. However, the existing aerogel felt needs to use supercritical drying in the preparation process. The device is expensive and energy-intensive, and the process preparation process of aerogel felt is long and the process control is imprecise, which can easily lead to unstable product insulation performance and low product qualification rate. In addition, the explosion temperature of a single battery cell of an existing ordinary new energy electric vehicle battery is between 350-650℃, and the high temperature tolerance of the insulation board of the battery cell is between 350-650℃, which can give personnel more than 15 minutes of safe escape time. Basically, there is no need to use an insulation board with a higher temperature tolerance as a battery cell insulation film, which can meet the use requirements. Summary of the invention

[0006] In view of this, the first object of the present invention is to provide a nano thermal insulation board, which is made by a dry method and has the characteristics of good thermal insulation performance, uniform texture, stable compression performance, long-term service with a maximum temperature range of 350-650 ° C, low production cost, etc., and is suitable for thermal insulation film for battery cells for ordinary electric vehicles.

[0007] In order to achieve the above-mentioned object, the present invention provides a nano thermal insulation board, which is mainly made of the following raw materials by mass through dry mixing, molding and hydrophobic treatment: 10-30 parts of hollow glass microspheres, 50-70 parts of thermal insulation powder, 5-20 parts of sunscreen, 2-10 parts of fiber and hydrophobic agent, wherein the amount of the hydrophobic agent is 30-180 kg / m based on the volume of the nano thermal insulation board. 3 .

[0008] The second object of the present invention is to provide a method for preparing the above-mentioned nano thermal insulation board, which has low production cost, and the prepared nano thermal insulation board has good thermal insulation performance and stable compression performance, and can effectively improve the safety of batteries for electric vehicles.

[0009] Specifically, a method for preparing a nano thermal insulation board comprises the following steps: Dry mix: first mix the insulation powder and hollow glass microspheres evenly, then add the fiber and sunscreen agent in sequence and mix evenly to form a mixture; Compression molding: taking 90-180 g of the mixture and using a flat vulcanizing machine to press and mold it to obtain a nano separator blank; Hydrophobic treatment: Vacuum vapor phase hydrophobic method is used, based on the volume of the nano separator blank, according to 30-180 kg / m 3 The nano insulation board blank is subjected to hydrophobic treatment using a hydrophobic agent in an amount of and then dried to obtain the nano insulation board.

[0010] The third object of the present invention is to provide an application of the above nano thermal insulation board in the preparation of a battery, which is used as a thermal insulation film for a battery cell. The battery is preferably a battery for new energy vehicles, and the explosion temperature of a single cell of the battery is 350-650°C.

[0011] Therefore, the nano thermal insulation board provided by the present invention is mainly prepared by a dry method, which does not require expensive drying equipment, and the raw materials for preparation are all mature large-scale industrial products on the market with low prices, thereby making the production cost of the nano thermal insulation board low; in addition, hollow glass microspheres with high fluidity are added to the raw materials of the present invention, while maintaining the thermal insulation performance of the nano thermal insulation board, it can also improve the uniformity of mass distribution of the mixture in the mold during the molding process, thereby improving the compression stability of the prepared sample. The above-mentioned nano thermal insulation board provided by the present invention has a density of 0.27-0.5 g / cm 3 , the standard error does not exceed 0.5%; the compression rates at 1 MPa and 2 MPa are 15%-40% and 30%-40% respectively; the hydrophobicity is not less than 99%, and the room temperature thermal conductivity is not higher than 0.03 W / (m·K), and the maximum temperature range for long-term service is 350-650 ℃. Therefore, the above-mentioned nano heat insulation board is applied to the battery and used as an electric vehicle battery insulation film, which can prevent the product from being damaged due to the unstable compression performance of the nano heat insulation board, and then lead the heat of the explosion to other batteries, that is, prevent the heat from causing other batteries to lose control, leaving at least 15 minutes of escape time for personnel, and the 15-minute escape time can meet the use of electric vehicles, reduce the destructive power of electric vehicle explosions, and have no fundamental damage to the vehicle body, thereby effectively improving the safety of heat outflow caused by battery cell failure; therefore, the above-mentioned nano heat insulation board provided by the present invention is suitable for battery cell insulation, especially as a battery cell insulation film for ordinary electric vehicle batteries, which can reduce the destructive power of electric vehicle explosions and will not cause destructive damage to the entire vehicle structure. DETAILED DESCRIPTION

[0012] The technical solution of the present invention is further described in detail below through specific implementation methods.

[0013] The terms used in the present invention are all commonly used terms in the relevant field. The raw materials, equipment, preparation processes, testing methods, etc. used are all prior arts in the relevant field unless otherwise specified.

[0014] The first object of the present invention is to provide a nano thermal insulation board which is made by a dry method and has the characteristics of good thermal insulation performance, uniform texture, stable compression performance, low production cost, etc.

[0015] In order to achieve the above object, the present invention provides a nano thermal insulation board, which is mainly made of the following raw materials by mass through dry mixing, molding and hydrophobic treatment: 10-30 parts of hollow glass microspheres, 50-70 parts of thermal insulation powder, 5-20 parts of sunscreen, 2-10 parts of fiber and hydrophobic agent, wherein the amount of the hydrophobic agent is 30-180kg / m based on the volume of the nano thermal insulation board. 3 .

[0016] The hollow glass microspheres have a series of excellent properties such as strong fluidity, low density, low dielectric constant, insolubility in water, acid and alkali resistance, and are a high-performance functional material. The main function of adding hollow glass microspheres in the present invention is to improve the fluidity of the raw material mixture in the preparation process of the nano thermal insulation board, so that the material distribution is more uniform during the spreading process, and the nano board has a relatively stable compression performance. Therefore, the hollow glass microspheres should have high fluidity, and the particle size is preferably 65-110 μm, and the true density is preferably 0.18-0.4 g / cm 3 ; Further, the model of the hollow glass microspheres is at least one of HL20, HL25, HL30, HL32 and HL38 of Zhengzhou Saint-Lite Hollow Microsphere New Materials Co., Ltd.; in this way, the hollow glass microspheres have good fluidity and a thicker wall thickness, can withstand high temperatures of 500-650°C for a short time, and have good thermal insulation performance.

[0017] If the amount of hollow glass microspheres is too much, the molding will not be formed; if the amount is too little, the material will not be evenly distributed. Therefore, the amount of hollow glass microspheres is preferably 10-30 parts.

[0018] The insulation powder as the main insulation material can be one of fumed silica, fumed alumina powder, silica aerogel powder or a mixture of the two, and its particle size is preferably 15-60 nm. If the amount of insulation powder is too much, the compression deformation of the insulation board at 1 MPa will be reduced; if the amount is too little, the strength of the sample will be reduced and the compression deformation at 1 MPa will be increased; therefore, the amount of insulation powder is preferably 50-70 parts.

[0019] The sunscreen is mainly used to suppress thermal radiation, and can be a mixture of one or more of silicon carbide, titanium dioxide, carbon black, potassium hexatitanate whiskers, zinc oxide, and zirconium oxide, and its particle size is preferably 1.5-4 μm. If the amount of sunscreen is too much, it is difficult to make the nano thermal insulation board adopt dry molding; if the amount is too little, the thermal insulation performance of the nano thermal insulation board will be reduced; therefore, the amount of sunscreen is preferably 5-20 parts.

[0020] The fibers are mainly used to improve the strength of the nano thermal insulation board and have a reinforcing effect. They can be a mixture of one or more of glass fiber, high silica fiber, basalt fiber, quartz fiber, and PP fiber. Preferably, the fiber has a diameter of 5-14 μm and a length of 2-12 mm. If the amount of fiber used is too much, it is easy to agglomerate and has poor fluidity, which makes it difficult to flatten the nano thermal insulation board during the spreading process when the nano thermal insulation board is made by the dry method, and even bulging may occur, resulting in uneven texture distribution of the nano thermal insulation board and unstable compression performance. If the amount used is too little, it is difficult to play a reinforcing role on the nano thermal insulation board. Therefore, the amount of fiber used is preferably 2-10 parts.

[0021] The hydrophobic agent is a prior art, and is mainly used to make the nano insulation board hydrophobic and prevent water molecules in the air (in the environment) from entering the nano board. Water is a good thermal conductor, which makes the insulation board lose its thermal insulation performance. Therefore, it can be hexamethyldisilazane, hexamethyldisilazane, methyltriethoxysilane, methyltrimethoxysilane, dimethyldiethoxysilane, dimethyldimethoxysilane. If the amount of hydrophobic agent is too much, it will lead to waste of hydrophobic agent raw materials and increase production costs; if the amount is too little, the hydrophobic performance of the sample will not meet the requirements. If the sample is used for a long time, the thermal insulation performance of the sample will decrease. In the specific construction process, the amount of hydrophobic agent can be determined according to the actual situation. Usually, the amount of hydrophobic agent is 30-180 kg / m 3 , preferably 50-150 kg / m 3 , such as 50 kg / m 3 , 60 kg / m 3 , 70 kg / m 3 , 80 kg / m 3 , 90 kg / m 3 , 100 kg / m 3 , 110 kg / m 3 , 120 kg / m 3 , 130 kg / m 3 , 140 kg / m 3 , 150 kg / m 3 wait.

[0022] The second object of the present invention is to provide a method for preparing the above-mentioned nano-insulation board, which has low production cost, and the prepared nano-insulation board has good thermal insulation performance and stable compression performance. Its maximum long-term service temperature range is 350-650 ° C. As a thermal insulation film for battery cells, it can effectively improve the safety of batteries for ordinary electric vehicles.

[0023] Specifically, a method for preparing a nano thermal insulation board comprises the following steps: Dry mix: first mix the insulation powder and hollow glass microspheres evenly, then add the fiber and sunscreen agent in sequence and mix evenly to form a mixture; Compression molding: weighing the mixed material and using a flat vulcanizing machine to press and mold it to obtain a nano separator blank; Hydrophobic treatment: Vacuum vapor phase hydrophobic method is used, based on the volume of the nano separator blank, according to 30-180 kg / m 3 The nano insulation board blank is treated with a hydrophobic agent in an amount of and then dried to obtain the nano insulation board.

[0024] The main purpose of the dry blend is to evenly mix all the raw materials to obtain a mixture with uniform texture, which specifically includes: firstly evenly mixing the insulation powder and hollow glass microspheres at 30-100 r / min; then adding the fiber for a second even mixing; and then adding the sunscreen for a third even mixing to form the mixture. The time for each even mixing is preferably 30-50 min.

[0025] The compression molding step includes weighing a quantitative amount of the mixture, pouring it into a flat plate vulcanizer pressing mold, flattening it with a tool, and then pre-exhausting it with an exhaust plate, and finally using an automated flat plate vulcanizer for compression molding to obtain a nano partition blank. Among them, since hollow glass microspheres are added to the mixture, the fluidity of the mixture can be greatly improved, so that the material distribution is more uniform during the spreading process, which is conducive to the preparation of a nano insulation board with relatively stable compression performance. The shape and size of the mold affect the shape and size of the nano insulation board, so the shape and size of the mold can be determined according to actual needs; preferably, the amount of the mixture is 100-180 g.

[0026] The hydrophobic treatment is a prior art, and the specific steps include: placing the nano separator blank in a vacuum drying oven with a vacuum degree of 0.05-0.09 MPa, at 120-180°C, weighing a hydrophobic agent based on the volume of the nano separator blank and placing it at the bottom of the vacuum drying oven, so that the amount of the hydrophobic agent is 30-180 kg / m 3 ; Then evacuate to a vacuum degree of 0.06 MPa, close the vacuum drying oven, and maintain drying at 120-180°C for 2-6 h.

[0027] The vacuum vapor phase hydrophobic method adopted by the present invention not only uses a small amount of hydrophobic agent, but also has the characteristics of short process cycle, safe and efficient operation, no waste liquid discharge, and compared with liquid phase hydrophobicity, the vapor phase hydrophobic process does not destroy the internal space structure of the material.

[0028] Therefore, the nano thermal insulation board provided by the present invention is mainly prepared by a dry method, which does not require expensive drying equipment and has a low production cost. In addition, hollow glass microspheres with high fluidity are added to the raw materials of the present invention, which can improve the thermal insulation performance of the nano thermal insulation board while also improving the uniformity of mass distribution of the mixture in the mold during the compression molding process, thereby improving the compression stability of the prepared sample. The density of the nano thermal insulation board provided by the present invention is 0.27-0.5 g / cm 3 , the standard error does not exceed 0.5%; the compression rates at 1 MPa and 2 MPa are 15%-40% and 30%-40% respectively; the hydrophobicity is not less than 99%, and the room temperature thermal conductivity is not higher than 0.03 W / (m·K), and the maximum temperature range for long-term service is 350-650 ℃.

[0029] Therefore, the application of the above nano thermal insulation board to batteries, as an insulation film for electric vehicle batteries, can effectively improve the safety of batteries that cause heat to flow out due to battery cell failure; therefore, the third object of the present invention is to provide an application of the above nano thermal insulation board in the preparation of batteries. Further, the application of the thermal insulation board in the preparation of the insulation film for the battery cell; preferably, the battery is a battery for electric vehicles.

[0030] The present invention will further illustrate the technical solution to be protected by the present invention with specific embodiments below.

[0031] Example 1 This embodiment provides a nano heat insulation board, which is prepared by dry mixing, compression molding and hydrophobic treatment; the specific preparation method includes the following steps: Dry mix: 20 parts of hollow glass microspheres HL20, 60 parts of fumed silica powder, 17 parts of silicon carbide, 3 parts of glass fiber and hexamethyldisilazane, according to the mass fraction. The amount of hexamethyldisilazane is 50 kg / m based on the volume of the nano thermal insulation board. 3 ; Add the above-mentioned fumed silica powder and hollow glass microspheres into a mixer and mix them. The mixing time is 40 min and the mixer speed is 40 r / min, so that the fumed silica powder and the hollow glass microspheres are evenly mixed; then add the glass fiber into the mixer and disperse and mix evenly at a speed of 30 r / min for 40 min; then add the sunscreen agent silicon carbide into the mixer and continue to disperse in the mixer at 40 r / min for 40 min to form a mixture; Compression molding: weigh 108g of the above mixture and pour it into a compression mold of a flat vulcanizer, flatten it using a tooling, then use a vent plate for pre-exhaust, and finally use an automated flat vulcanizer for compression molding to obtain a nano separator blank; Hydrophobic treatment: Place the nano separator blank in a vacuum drying oven at a temperature of 150°C and use a hydrophobic agent at a dosage of 50 kg / m 3 , add the hydrophobic agent hexamethyldisilazane, weigh a certain amount of the hydrophobic agent and place it at the bottom of the vacuum drying oven, then evacuate the oven to a vacuum degree of 0.08 MPa, close the vacuum drying oven, and keep drying at 150°C for 3 h.

[0032] Example 2 This embodiment provides a nano heat insulation board, which is prepared by dry mixing, compression molding and hydrophobic treatment; the specific preparation method includes the following steps: Dry mix: 10 parts of hollow glass microspheres HL30, 65 parts of fumed alumina powder, 14 parts of titanium dioxide, 6 parts of basalt fiber and hexamethyldisilazane, wherein the amount of hexamethyldisilazane is 100 kg / m based on the volume of the nano thermal insulation board. 3 ; Add the above-mentioned fumed alumina powder and hollow glass microspheres into a mixer and mix them for 40 minutes at a mixer speed of 60 r / min, so that the fumed alumina powder and the hollow glass microspheres are evenly mixed; then add basalt fiber into the mixer and disperse and mix evenly at a speed of 70 r / min for 40 minutes; then add the sunscreen titanium dioxide into the mixer and continue to disperse in the mixer at 70 r / min for 40 minutes to form a mixture; Compression molding: Weigh 139 g of the above mixture and pour it into a flat-plate vulcanizer pressing mold, flatten it using a tooling, then use a vent plate for pre-venting, and finally use an automated flat-plate vulcanizer for compression molding to obtain a nano separator blank.

[0033] Hydrophobic treatment: Place the nano separator blank in a vacuum drying oven at 150°C and heat at a hydrophobic dosage of 100 kg / m 3 , add the hydrophobic agent hexamethyldisilazane, weigh a certain amount of the hydrophobic agent and place it at the bottom of the vacuum drying oven, then evacuate the vacuum oven to reach a vacuum degree of 0.06 MPa, close the vacuum drying oven, and keep drying at 150°C for 4 h.

[0034] Example 3 This embodiment provides a nano heat insulation board, which is prepared by dry mixing, compression molding and hydrophobic treatment; the specific preparation method includes the following steps: Dry mix: 30 parts of hollow glass microspheres HL38, 55 parts of silica aerogel powder, 6 parts of zinc oxide, 9 parts of high silica fiber and methyl trimethoxy silane, according to the mass fraction. The amount of methyl trimethoxy silane is 150 kg / m based on the volume of the nano thermal insulation board. 3 ; Add the above-mentioned silica aerogel powder and hollow glass microspheres into a mixer and mix them for 40 min at a mixer speed of 90 r / min, so that the silica aerogel powder and the hollow glass microspheres are evenly mixed; then add methyltrimethoxysilane into the mixer, disperse and mix evenly for 40 min at a speed of 40 r / min; then add the sunscreen zinc oxide into the mixer, and continue to disperse in the mixer at 90 r / min for 40 min to form a mixture; Compression molding: Weigh 172 g of the above mixture and pour it into a flat-plate vulcanizer pressing mold, flatten it using a tooling, then use a vent plate for pre-venting, and finally use an automated flat-plate vulcanizer for compression molding to obtain a nano separator blank.

[0035] Hydrophobic treatment: Place the nano separator blank in a vacuum drying oven at 150°C and add a hydrophobic dose of 150 kg / m 3 , add hydrophobic agent methyltrimethoxysilane, weigh a certain amount of hydrophobic agent and place it at the bottom of the vacuum drying oven, then evacuate the oven to a vacuum degree of 0.07 MPa, close the vacuum drying oven, and keep drying at 150°C for 5 h.

[0036] The present invention also provides an application of the nano heat insulation board provided in the above-mentioned embodiments 1, 2 and 3 as a heat insulation film in an electric vehicle battery.

[0037] Comparative Example Comparative Example 1 provides a nano thermal insulation board, which is substantially the same as the nano thermal insulation board provided in Example 1, with the main differences being: no hollow glass microspheres are added in this comparative example, and other raw materials and process steps remain unchanged; Comparative Example 2 provides a nano heat insulation board, which is basically the same as the nano heat insulation board provided in Example 2, with the main difference being that in this comparative example, white carbon black powder with the same solid content is used to replace the hollow glass microspheres in Example 2, and other raw materials and process steps remain unchanged; Comparative Example 3 provides a nano thermal insulation board, which is basically the same as the nano thermal insulation board provided in Example 3, with the main difference being that in this comparative example, microsilica powder with the same solid content is used to replace the hollow glass microspheres in Example 3, and other raw materials and process steps remain unchanged; Comparative Example 4 provides a nano thermal insulation board, which is basically the same as the nano thermal insulation board provided in Example 1, with the main differences being: the amount of hollow glass microspheres used in this comparative example is 40 parts, and other raw materials and process steps remain unchanged; Comparative Example 5 provides a nano-insulation board, which is basically the same as the nano-insulation board provided in Example 1, with the main differences being: this comparative example adopts a liquid phase hydrophobic process, and the amount of hydrophobic agent used is the same as that in Example 1, and alcohol is used to dilute it to the same volume as the felt, and the height is controlled with a grid mesh, maintained at 50°C for 4 hours, and then the sample is taken out and dried at 100°C for 2 hours, while the other parts remain unchanged.

[0038] Comparative Example 6 provides a nano thermal insulation board, which is basically the same as the nano thermal insulation board provided in Example 2, with the main differences being: the amount of basalt fiber used in this comparative example is 1 part, and other raw materials and process steps remain unchanged; Comparative Example 7 provides a nano thermal insulation board, which is basically the same as the nano thermal insulation board provided in Example 2, with the main difference being that the amount of basalt fiber used in this comparative example is 15 parts, and other raw materials and process steps remain unchanged.

[0039] Performance Testing The nano thermal insulation boards provided in Examples 1-3 and Comparative Examples 1-7 were used as test samples for fluidity, quality, thermal insulation performance, compression performance, hydrophobic performance, etc. The results are shown in Table 1-2. The size of the mold used in the preparation process of the above test samples is 350 mm×325 mm×3 mm, so the size of each test sample is 350 mm×325 mm×3 mm.

[0040] Fluidity test: During the compression molding process of the mixture formed during the preparation of the above test samples, the fluidity of the corresponding mixture is tested using a powder comprehensive properties tester, and the fluidity of the mixture is described by testing the Carr fluidity index. The larger the Carr fluidity index, the better the fluidity of the dry mixture.

[0041] Quality test: The size of the test sample for the compression performance of each part of the test sample is 60 mm×60 mm×3 mm. Each test sample is cut into 25 compression performance test samples, and the number of samples for statistical quality deviation is 72. The maximum and minimum values ​​are counted, and the mean and standard deviation are calculated. The smaller the standard deviation, the better the quality of the test sample and the more uniform the distribution of the mixture.

[0042] Thermal insulation performance test: Use Mitutoyo 547-301 thickness gauge to test the initial thickness of the sample 1; set the heater temperature to 650℃ and start heating; after the heater temperature stabilizes at 650℃, quickly place the insulation pad on the heating table, then arrange the thick aluminum block and pressure sensor, apply a stress of 0.9 MPa, start timing, with a time interval of 1s, and use a plug gauge to detect the thickness 2 after 2 minutes; after 5 minutes, release the pressure to 0.03 MPa, use a plug gauge to detect the thickness 3, and calculate the thickness retention rate; use a plug gauge to detect the thickness after 10 minutes, and use a plug gauge to detect the thickness after 20 minutes; export the temperature data during the test, and record the hot surface-cold surface temperature difference data after 20 minutes.

[0043] The compression performance and hydrophobic performance were tested with reference to the national standard GB T34336-2017 (nanoporous aerogel composite insulation products).

[0044] Thermal conductivity test: Refer to GB / T 10295-2008 Determination of Steady-State Thermal Resistance and Related Properties of Insulating Materials by Heat Flow Meter Method, and use the thermal conductivity tester JW-Ш made by China Academy of Building Research to test the samples. The test was carried out under the environment of temperature 25±2℃ and humidity 50%RH-70%RH. The size of the sample to be tested was 300×300×3㎜, and the number was 3. The thickness of each part of each sample was tested, and then the average thickness was calculated.

[0045] Table 1 Test results of stability and flow properties of nano thermal insulation board Table 2 Nano-insulation board hydrophobicity and thermal insulation performance test results Combining Table 1-2, we can draw the following conclusions: 1) It can be seen from Example 1 and Comparative Example 1, Example 2 and Comparative Example 2, and Example 3 and Comparative Example 3 that adding hollow glass microspheres in the process of dry-process nano-insulation board can effectively improve the quality uniformity and fluidity of the nano-insulation board. This is mainly because the introduction of hollow glass microspheres with good fluidity as carriers makes the mixed material evenly distributed, while white carbon black and microsilica powder have good thermal insulation properties, but poor fluidity, so the mixed material cannot be evenly distributed.

[0046] 2) By comparing Example 1 and Comparative Example 5, it is found that the nano thermal insulation board provided in Comparative Example 5 is denser and has an increased density after liquid-phase hydrophobic treatment. This may be because liquid enters the pore structure of the nano thermal insulation board. During the drying process, due to the evaporation of the hydrophobic agent, the capillary force will cause the pore structure to collapse, the porosity of the sample will decrease, and the density of the sample will increase. Therefore, under the premise that other conditions are the same, the hydrophobicity of the nano thermal insulation board provided in Comparative Example 5 is 86.4%, and the sample has a long hydrophobic period, which is not conducive to production efficiency.

[0047] 3) By comparing Example 1, Comparative Example 1 and Comparative Example 4, it is found that without adding hollow glass microspheres, the quality uniformity and compression performance of the nano thermal insulation board provided by Comparative Example 1 are relatively poor; if excessive hollow glass microspheres are added, the powder material cannot be formed in the subsequent compression molding process; this is mainly because the hollow glass microspheres have good fluidity and good high temperature resistance, so the addition of hollow glass microspheres should be appropriate, preferably limited to 10-30 parts by mass.

[0048] 4) Comparison of Example 2, Comparative Example 6 and Comparative Example 7 shows that: when the amount of fiber is small, the fluidity becomes better, but the strength of the prepared sample is weak; when the amount of fiber is high, the fibers will agglomerate with each other, resulting in a large difference in the composition of the mixed material; this is mainly because of the synergistic effect between the thermal insulation powder, infrared sunscreen and fiber. The thermal insulation powder can effectively separate the fibers within the appropriate dosage range. When the amount of fiber is too large, the amount of thermal insulation powder is insufficient to separate the fibers, resulting in bulges in the sample due to fiber agglomeration. Therefore, the fiber should be added in an appropriate amount, preferably limited to 2-10 parts by mass.

[0049] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, ordinary technicians in the field should understand that the specific implementation methods of the present invention can still be modified or some technical features can be replaced by equivalents without departing from the spirit of the technical solution of the present invention, which should be included in the scope of the technical solution for protection of the present invention.

Claims

1. A nano thermal insulation board, characterized in that: The nano thermal insulation board is mainly prepared by dry mixing, molding and hydrophobic treatment of the following raw materials: 10-30 parts of hollow glass microspheres, 50-70 parts of thermal insulation powder, 5-20 parts of sunscreen, 2-10 parts of fiber and hydrophobic agent, wherein the amount of the hydrophobic agent is 30-180 kg / m 3 .

2. The nano thermal insulation board according to claim 1, characterized in that: The hollow glass microspheres have a particle size of 65-110 μm and a true density of 0.18-0.4 g / cm 3 .

3. The nano heat insulation board according to claim 1 or 2, characterized in that: The heat-insulating powder is one or a mixture of fumed silica, fumed alumina powder and silica aerogel powder; Preferably, the particle size of the thermal insulation powder is 15-60 nm.

4. The nano heat insulation board according to claim 1 or 2, characterized in that: The sunscreen is a mixture of one or more of silicon carbide, titanium dioxide, carbon black, potassium hexatitanate whiskers, zinc oxide and zirconium oxide; Preferably, the particle size of the sunscreen agent is 1.5-4 μm.

5. The nano heat insulation board according to claim 1 or 2, characterized in that: The fiber is one of glass fiber, high silica fiber, basalt fiber, quartz fiber and PP fiber, or a mixture of any combination; Preferably, the fiber has a diameter of 5-14 μm and a length of 2-12 mm.

6. A method for preparing the nano thermal insulation board according to any one of claims 1 to 5, comprising the following steps: Dry mix: first mix the insulation powder and hollow glass microspheres evenly, then add the fiber and sunscreen agent in sequence and mix evenly to form a mixture; Compression molding: weighing the mixed material and using a flat vulcanizing machine to press and mold it to obtain a nano separator blank; Hydrophobic treatment: Vacuum vapor phase hydrophobic method is used, based on the volume of the nano separator blank, according to 30-180 kg / m 3 The nano insulation board blank is subjected to hydrophobic treatment using a hydrophobic agent in an amount of and then dried to obtain the nano insulation board.

7. The preparation method according to claim 6, characterized in that: The dry mixing step comprises: firstly, uniformly mixing the heat insulation powder and hollow glass microspheres at 30-100 r / min; then, adding the fiber and uniformly mixing them for a second time; and then, adding the sunscreen agent and uniformly mixing them for a third time to form the mixture; Preferably, each uniform mixing time is 30-50 min.

8. The preparation method according to claim 6 or 7, characterized in that: The compression molding step includes weighing a certain amount of the mixture, pouring it into a compression mold of a flat vulcanizer, flattening it using a tool, then pre-exhausting it using an exhaust plate, and finally compression molding it using an automated flat vulcanizer to obtain a nano separator blank; Preferably, the amount of the mixed material is 100-180 g.

9. The preparation method according to claim 1 or 6, characterized in that: The hydrophobic treatment step comprises: placing the nano separator blank in a vacuum drying oven with a vacuum degree of 0.05-0.09 MPa, weighing a hydrophobic agent based on the volume of the nano separator blank and placing it at the bottom of the vacuum drying oven at 120-180° C., so that the amount of the hydrophobic agent is 30-180 kg / m 3 ; Then evacuate to a vacuum degree of 0.06 MPa, close the vacuum drying oven, and keep drying at 120-180°C for 2-6 h; Preferably, the amount of the hydrophobic agent is 50-150 kg / m 3 .

10. Use of the nano heat insulation board according to any one of claims 1 to 5 in preparing a battery; Preferably, the heat insulation board is used in preparing the heat insulation film of the battery cell; Preferably, the battery is a battery for electric vehicles.

Citation Information

Patent Citations

  • High-efficiency heat-insulation flame-retardant material between single battery cells