Photocuring formed ceramic slurry and preparation method thereof

By preparing ceramic powder composites and performing surface modification treatment, the problem of poor fit of ceramic powder is solved, the mechanical properties and long-term stability of ceramic materials are improved, and the high mechanical properties and long-term storage of ceramic slurries are achieved. ability.

CN119080481APending Publication Date: 2024-12-06HENAN XINGXING PIPELINE ENG TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411203421.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The coordination effect between existing ceramic powders is not ideal, which affects the sedimentation performance and long-term use effect of the slurry, resulting in insufficient mechanical properties of the ceramic materials.

Method used

By preparing ceramic powder composites, different particle size combinations of alumina powder and yttrium oxide powder are used, and surface modification is performed on large-sized alumina powders, and the suspension capacity is adjusted in combination with modified polyethylene glycol. Form a uniform and tight powder structure.

Benefits of technology

The high mechanical properties and long-term stability of ceramic slurries are achieved, resource waste is reduced, labor costs are saved, and the solid phase content and molding performance of ceramic products are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005018365530000141
    Figure BDA0005018365530000141
Patent Text Reader

Abstract

The invention relates to a photocuring molded ceramic slurry and a preparation method thereof, and belongs to the technical field of ceramic slurry, the photocuring molded ceramic slurry comprises the following components by weight: 65-75 parts of a ceramic powder compound, 24-26 parts of dipentaerythritol hexaacrylate, 0.2-0.4 part of a photoinitiator, 0.4-0.6 part of a dispersant, 1.0-1.4 parts of an antifoaming agent and 2.5-3.5 parts of modified polyethylene glycol; the ceramic slurry prepared by the invention has beneficial mechanical properties, can be placed for a long time, reduces the waste of resources, and saves the labor cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic slurries, and in particular to a photocurable ceramic slurry and a preparation method thereof. Background Art

[0002] In photocuring ceramic slurry, combining ceramic powders of different particle sizes can improve the compactness of the powder, thereby improving the mechanical properties of the ceramic material.

[0003] However, the coordination effect between ceramic powders in the prior art is not ideal. In addition, since ceramic powders of different particle sizes have different suspension capabilities, the sedimentation performance of the slurry is affected to a certain extent, resulting in a shorter placement time of the slurry, which affects the long-term use effect of the slurry. Summary of the invention

[0004] 1. Technical issues to be solved

[0005] In view of the deficiencies in the prior art, the present invention provides a photocurable ceramic slurry and a preparation method thereof.

[0006] (II) Technical solution

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0008] A photocurable ceramic slurry comprises the following components by weight: 65-75 parts of a ceramic powder compound, 24-26 parts of dipentaerythritol hexaacrylate, 0.2-0.4 parts of a photoinitiator, 0.4-0.6 parts of a dispersant, 1.0-1.4 parts of a defoamer and 2.5-3.5 parts of modified polyethylene glycol.

[0009] Furthermore, the method for preparing the ceramic powder composite comprises the following steps:

[0010] S 1 : Weigh alumina powder and yttrium oxide powder, wherein the mass ratio of alumina powder to yttrium oxide powder is (20-30):3;

[0011] S 2 : Place the alumina powder in a pickling solution 10 to 15 times the weight of the alumina powder, treat it in a water bath at 40 to 50°C for 4 to 8 hours, wash it with clean water after the treatment, filter it, and dry it to obtain the pickled alumina powder;

[0012] S 3 : Add 0.6-1.0% of the surface modifier by weight of the alumina powder to the acid-washed alumina powder, use 2-5 times the weight of the alumina powder as anhydrous ethanol as a medium, mix in a reactor for 2-3 hours, filter and dry after mixing to obtain pretreated alumina powder;

[0013] S 4 : The obtained pretreated alumina powder is placed in a reactor, 8 to 12% of the mass of the alumina powder is added with isobornyl methacrylate, stirred for 0.5 to 1 hour to obtain modified alumina powder, and then yttrium oxide powder is added and stirred for 20 to 30 minutes to finally obtain a ceramic powder composite.

[0014] Furthermore, the particle size of the aluminum oxide powder is 6 to 10 μm, and the particle size of the yttrium oxide powder is 0.25 to 1 μm.

[0015] Furthermore, the pickling solution is a mixture of hydrochloric acid solution and lithium fluoride, and the mass ratio of hydrochloric acid solution to lithium fluoride is (20-30):3.

[0016] Furthermore, the volume concentration of the hydrochloric acid solution is 30-40%.

[0017] Furthermore, the surface modifier is KH560.

[0018] Furthermore, the photoinitiator is phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, the dispersant is BYK111, and the defoaming agent is polydimethylsiloxane.

[0019] Furthermore, the preparation method of the modified polyethylene glycol comprises the following steps:

[0020] A 1 : By weight, 3 to 5 parts of lignin are added into the reactor, followed by 6 to 8 parts of dimethylaminoethyl methacrylate and 60 parts of polyethylene glycol-400, stirring is started, and the mixture is heated to 50 to 60° C. and reacted for 1 to 1.5 hours. After the reaction is completed, an intermediate product is obtained;

[0021] A 2 The intermediate product is washed with water and rotary evaporated at a temperature of 80 to 85°C, a pressure of 5 to 7 hPa, and a time of 0.5 to 1 h, and then activated carbon is added for adsorption and decolorization to obtain modified polyethylene glycol.

[0022] A method for preparing a photocurable ceramic slurry comprises the following steps:

[0023] B 1 : Take ceramic powder composite, dipentaerythritol hexaacrylate, photoinitiator, dispersant and modified polyethylene glycol respectively by weight, mix them evenly and heat to 50-70° C., add defoamer and stir for 0.5-1h to obtain slurry premix;

[0024] B 2 : Transfer the slurry premix to the reactor, stir for 4 to 6 hours, discharge the material, and obtain the light-cured ceramic slurry, wherein the rotation speed is 150 to 200 r / min.

[0025] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:

[0026] 1. The ceramic mixed powder provided by the present invention comprises large-particle alumina powder and small-particle yttrium oxide powder. The large-particle alumina powder is treated separately to coat its surface with isobornyl methacrylate, and then the modified polyethylene glycol is regulated to finally achieve a balance in the suspension capacity of the large-particle alumina powder and the small-particle yttrium oxide powder, thereby avoiding the generation of sedimentation.

[0027] In addition, the modified alumina powder has a certain amount of activity space in the slurry, which can improve the coordination effect between it and the yttrium oxide powder, and is beneficial to the uniform and tight arrangement of the modified alumina powder and the yttrium oxide powder during the photocuring process. Finally, the two powders of different particle sizes form a graded and dense structure, so that the final ceramic product has higher mechanical properties.

[0028] 2. The present invention provides a photocurable ceramic slurry having good slurry viscosity and high solid content, good slurry forming performance, and high mechanical strength of ceramic products.

[0029] At the same time, the ceramic slurry prepared by the present invention has high long-term stability and can be stored for a long time, thereby reducing waste of resources and saving labor costs. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] In the following examples and comparative examples: the surface modifier is KH560, the photoinitiator is phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, the dispersant is BYK111, and the defoamer is polydimethylsiloxane.

[0032] Example 1

[0033] A photocurable ceramic slurry comprises the following components by weight: 65 parts of a ceramic powder compound, 24 parts of dipentaerythritol hexaacrylate, 0.2 parts of a photoinitiator, 0.4 parts of a dispersant, 1.0 parts of a defoamer and 2.5 parts of modified polyethylene glycol.

[0034] The method for preparing a ceramic powder composite comprises the following steps:

[0035] S 1 : Weigh alumina powder and yttrium oxide powder, wherein the mass ratio of alumina powder to yttrium oxide powder is 20:3;

[0036] S 2 : Place the alumina powder in an acid wash solution 10 times the weight of the alumina powder, treat it in a 40°C water bath for 4 hours, wash it with clean water after the treatment, filter it, and dry it to obtain the acid washed alumina powder;

[0037] S 3 : Add 0.6% of the surface modifier by weight of the alumina powder to the acid-washed alumina powder, use anhydrous ethanol twice the weight of the alumina powder as a medium, mix in a reactor for 2 hours, filter and dry after mixing to obtain pretreated alumina powder;

[0038] S 4 : The obtained pretreated alumina powder was placed in a reactor, 8% of isobornyl methacrylate by weight of the alumina powder was added, and stirred for 0.5 h to obtain modified alumina powder, and then yttrium oxide powder was added and stirred for 20 min to finally obtain a ceramic powder composite.

[0039] The particle size of the aluminum oxide powder is 6 μm, and the particle size of the yttrium oxide powder is 0.25 μm.

[0040] The pickling solution is a mixture of hydrochloric acid solution and lithium fluoride, and the mass ratio of the hydrochloric acid solution to the lithium fluoride is 20:3.

[0041] The volume concentration of the hydrochloric acid solution is 30%.

[0042] The preparation method of modified polyethylene glycol comprises the following steps:

[0043] A 1 : By weight, 3 parts of lignin were added into the reactor, followed by 6 parts of dimethylaminoethyl methacrylate and 60 parts of polyethylene glycol-400, stirring was started, and the mixture was heated to 50° C. for 1 hour to obtain an intermediate product after the reaction was completed;

[0044] A 2 The intermediate product is washed with water and rotary evaporated at a rotary evaporation temperature of 80°C, a rotary evaporation pressure of 5hPa, and a rotary evaporation time of 0.5h, and then activated carbon is added for adsorption and decolorization to obtain modified polyethylene glycol.

[0045] A method for preparing a photocurable ceramic slurry comprises the following steps:

[0046] B 1: Take ceramic powder composite, dipentaerythritol hexaacrylate, photoinitiator, dispersant and modified polyethylene glycol respectively by weight, mix them evenly and heat to 50°C.

[0047] Add defoamer and stir for 0.5h to obtain slurry premix;

[0048] B 2 : The slurry premix was transferred into the reactor, stirred for 4 hours, and discharged to obtain the light-cured ceramic slurry, wherein the rotation speed was 150 r / min.

[0049] Example 2

[0050] A photocurable ceramic slurry comprises the following components by weight: 75 parts of a ceramic powder compound, 26 parts of dipentaerythritol hexaacrylate, 0.4 parts of a photoinitiator, 0.6 parts of a dispersant, 1.4 parts of a defoamer and 3.5 parts of modified polyethylene glycol.

[0051] The method for preparing a ceramic powder composite comprises the following steps:

[0052] S 1 : Weigh alumina powder and yttrium oxide powder, wherein the mass ratio of alumina powder to yttrium oxide powder is 10:1;

[0053] S 2 : Place the alumina powder in a pickling solution 15 times the weight of the alumina powder, treat it in a 50°C water bath for 8 hours, wash it with clean water after the treatment, filter it, and dry it to obtain the pickled alumina powder;

[0054] S 3 : Add 1.0% of the surface modifier by weight of the alumina powder to the acid-washed alumina powder, use 5 times the weight of the alumina powder as anhydrous ethanol as a medium, mix in a reactor for 3 hours, filter and dry after the mixing is completed to obtain pretreated alumina powder;

[0055] S 4 : The obtained pretreated alumina powder was placed in a reactor, and 12% of the mass of alumina powder was added with isobornyl methacrylate, and stirred for 1 hour to obtain modified alumina powder. Then, yttrium oxide powder was added and stirred for 30 minutes to finally obtain a ceramic powder composite.

[0056] The particle size of the aluminum oxide powder is 10 μm, and the particle size of the yttrium oxide powder is 1 μm.

[0057] The pickling solution is a mixture of hydrochloric acid solution and lithium fluoride, and the mass ratio of the hydrochloric acid solution to the lithium fluoride is 10:1.

[0058] The volume concentration of the hydrochloric acid solution is 40%.

[0059] The preparation method of modified polyethylene glycol comprises the following steps:

[0060] A 1 : By weight, 5 parts of lignin were added into the reactor, followed by 8 parts of dimethylaminoethyl methacrylate and 60 parts of polyethylene glycol-400, stirring was started, and the mixture was heated to 60° C. for 1.5 hours to obtain an intermediate product after the reaction was completed;

[0061] A 2 The intermediate product is washed with water and rotary evaporated at a rotary evaporation temperature of 85°C, a rotary evaporation pressure of 7hPa, and a rotary evaporation time of 1h, and then activated carbon is added for adsorption and decolorization to obtain modified polyethylene glycol.

[0062] A method for preparing a photocurable ceramic slurry comprises the following steps:

[0063] B 1 : Take ceramic powder composite, dipentaerythritol hexaacrylate, photoinitiator, dispersant and modified polyethylene glycol respectively by weight, mix them evenly and heat to 70°C.

[0064] Add defoamer and stir for 1 hour to obtain slurry premix;

[0065] B 2 : The slurry premix was transferred into the reactor, stirred for 6 hours, and discharged to obtain the light-cured ceramic slurry, wherein the rotation speed was 200 r / min.

[0066] Example 3

[0067] A photocurable ceramic slurry comprises the following components by weight: 70 parts of a ceramic powder compound, 25 parts of dipentaerythritol hexaacrylate, 0.3 parts of a photoinitiator, 0.5 parts of a dispersant, 1.2 parts of a defoamer and 3.0 parts of modified polyethylene glycol.

[0068] The method for preparing a ceramic powder composite comprises the following steps:

[0069] S 1 : Weigh alumina powder and yttrium oxide powder, wherein the mass ratio of alumina powder to yttrium oxide powder is 25:3;

[0070] S 2 : Place the alumina powder in a pickling solution 12 times the weight of the alumina powder, treat it in a 40°C water bath for 8 hours, wash it with clean water after the treatment, filter it, and dry it to obtain the pickled alumina powder;

[0071] S 3: Add 0.8% of the surface modifier by weight of the alumina powder to the acid-washed alumina powder, use anhydrous ethanol 3 times the weight of the alumina powder as the medium, mix in a reactor for 2 hours, filter and dry after the mixing is completed to obtain pretreated alumina powder;

[0072] S 4 : The obtained pretreated alumina powder was placed in a reactor, and 10% of the mass of the alumina powder was added with isobornyl methacrylate, and stirred for 0.5 h to obtain modified alumina powder. Then, yttrium oxide powder was added and stirred for 20 min to finally obtain a ceramic powder composite.

[0073] The particle size of the aluminum oxide powder is 8 μm, and the particle size of the yttrium oxide powder is 0.6 μm.

[0074] The pickling solution is a mixture of hydrochloric acid solution and lithium fluoride, and the mass ratio of the hydrochloric acid solution to the lithium fluoride is 25:3.

[0075] The volume concentration of the hydrochloric acid solution is 35%.

[0076] The preparation method of modified polyethylene glycol comprises the following steps:

[0077] A 1 : By weight, 4 parts of lignin were added into the reactor, followed by 7 parts of dimethylaminoethyl methacrylate and 60 parts of polyethylene glycol-400, stirring was started, and the mixture was heated to 50° C. and reacted for 1.5 hours. After the reaction was completed, an intermediate product was obtained;

[0078] A 2 The intermediate product is washed with water and rotary evaporated at a rotary evaporation temperature of 80°C, a rotary evaporation pressure of 7hPa, and a rotary evaporation time of 0.8h, and then activated carbon is added for adsorption and decolorization to obtain modified polyethylene glycol.

[0079] A method for preparing a photocurable ceramic slurry comprises the following steps:

[0080] B 1 : Take ceramic powder composite, dipentaerythritol hexaacrylate, photoinitiator, dispersant and modified polyethylene glycol respectively by weight, mix them evenly and heat to 60°C.

[0081] Add defoamer and stir for 0.5h to obtain slurry premix;

[0082] B 2 : The slurry premix was transferred into the reactor, stirred for 5 hours, and discharged to obtain the light-cured ceramic slurry, wherein the rotation speed was 180 r / min.

[0083] Comparative Example 1

[0084] The difference from Example 3 is that in the preparation of the ceramic powder composite, isobornyl methacrylate was not added in the treatment of step 4.

[0085] A photocurable ceramic slurry comprises the following components by weight: 70 parts of a ceramic powder compound, 25 parts of dipentaerythritol hexaacrylate, 0.3 parts of a photoinitiator, 0.5 parts of a dispersant, 1.2 parts of a defoamer and 3.0 parts of modified polyethylene glycol.

[0086] The method for preparing a ceramic powder composite comprises the following steps:

[0087] S 1 : Weigh alumina powder and yttrium oxide powder, wherein the mass ratio of alumina powder to yttrium oxide powder is 25:3;

[0088] S 2 : Place the alumina powder in a pickling solution 12 times the weight of the alumina powder, treat it in a 40°C water bath for 8 hours, wash it with clean water after the treatment, filter it, and dry it to obtain the pickled alumina powder;

[0089] S 3 : Add 0.8% of the surface modifier by weight of the alumina powder to the acid-washed alumina powder, use anhydrous ethanol 3 times the weight of the alumina powder as the medium, mix in a reactor for 2 hours, filter and dry after the mixing is completed to obtain pretreated alumina powder;

[0090] S 4 : The obtained pretreated alumina powder was placed in a reactor and stirred for 0.5 h to obtain modified alumina powder, and then yttrium oxide powder was added and stirred for 20 min to finally obtain a ceramic powder composite.

[0091] The particle size of the aluminum oxide powder is 8 μm, and the particle size of the yttrium oxide powder is 0.6 μm.

[0092] The pickling solution is a mixture of hydrochloric acid solution and lithium fluoride, and the mass ratio of the hydrochloric acid solution to the lithium fluoride is 25:3.

[0093] The volume concentration of the hydrochloric acid solution is 35%.

[0094] The preparation method of modified polyethylene glycol comprises the following steps:

[0095] A 1 : By weight, 4 parts of lignin were added into the reactor, followed by 7 parts of dimethylaminoethyl methacrylate and 60 parts of polyethylene glycol-400, stirring was started, and the mixture was heated to 50° C. and reacted for 1.5 hours. After the reaction was completed, an intermediate product was obtained;

[0096] A 2The intermediate product is washed with water and rotary evaporated at a rotary evaporation temperature of 80°C, a rotary evaporation pressure of 7hPa, and a rotary evaporation time of 0.8h, and then activated carbon is added for adsorption and decolorization to obtain modified polyethylene glycol.

[0097] A method for preparing a photocurable ceramic slurry comprises the following steps:

[0098] B 1 : Take ceramic powder composite, dipentaerythritol hexaacrylate, photoinitiator, dispersant and modified polyethylene glycol respectively by weight, mix them evenly and heat to 60°C.

[0099] Add defoamer and stir for 0.5h to obtain slurry premix;

[0100] B 2 : The slurry premix was transferred into the reactor, stirred for 5 hours, and discharged to obtain the light-cured ceramic slurry, wherein the rotation speed was 180 r / min.

[0101] Comparative Example 2

[0102] The difference from Example 3 is that in the preparation of the ceramic powder composite, the alumina powder is neither acid washed nor pretreated.

[0103] A photocurable ceramic slurry comprises the following components by weight: 70 parts of a ceramic powder compound, 25 parts of dipentaerythritol hexaacrylate, 0.3 parts of a photoinitiator, 0.5 parts of a dispersant, 1.2 parts of a defoamer and 3.0 parts of modified polyethylene glycol.

[0104] The method for preparing a ceramic powder composite comprises the following steps:

[0105] S 1 : Weigh alumina powder and yttrium oxide powder, wherein the mass ratio of alumina powder to yttrium oxide powder is 25:3;

[0106] S 2 : Alumina powder and yttrium oxide powder are placed in a reactor and mixed evenly, 10% of the mass of alumina powder isobornyl methacrylate is added, and stirred for 0.5 h to finally obtain a ceramic powder composite.

[0107] The particle size of the aluminum oxide powder is 8 μm, and the particle size of the yttrium oxide powder is 0.6 μm.

[0108] The preparation method of modified polyethylene glycol comprises the following steps:

[0109] A 1: By weight, 4 parts of lignin were added into the reactor, followed by 7 parts of dimethylaminoethyl methacrylate and 60 parts of polyethylene glycol-400, stirring was started, and the mixture was heated to 50° C. and reacted for 1.5 hours. After the reaction was completed, an intermediate product was obtained;

[0110] A 2 The intermediate product is washed with water and rotary evaporated at a rotary evaporation temperature of 80°C, a rotary evaporation pressure of 7hPa, and a rotary evaporation time of 0.8h, and then activated carbon is added for adsorption and decolorization to obtain modified polyethylene glycol.

[0111] A method for preparing a photocurable ceramic slurry comprises the following steps:

[0112] B 1 : Take ceramic powder composite, dipentaerythritol hexaacrylate, photoinitiator, dispersant and modified polyethylene glycol respectively by weight, mix them evenly and heat to 60°C.

[0113] Add defoamer and stir for 0.5h to obtain slurry premix;

[0114] B 2 : The slurry premix was transferred into the reactor, stirred for 5 hours, and discharged to obtain the light-cured ceramic slurry, wherein the rotation speed was 180 r / min.

[0115] Comparative Example 3

[0116] Different from Example 3, the polyethylene glycol was not modified.

[0117] A photocurable ceramic slurry comprises the following components by weight: 70 parts of a ceramic powder compound, 25 parts of dipentaerythritol hexaacrylate, 0.3 parts of a photoinitiator, 0.5 parts of a dispersant, 1.2 parts of a defoamer and 3.0 parts of polyethylene glycol.

[0118] The method for preparing a ceramic powder composite comprises the following steps:

[0119] S 1 : Weigh alumina powder and yttrium oxide powder, wherein the mass ratio of alumina powder to yttrium oxide powder is 25:3;

[0120] S 2 : Place the alumina powder in a pickling solution 12 times the weight of the alumina powder, treat it in a 40°C water bath for 8 hours, wash it with clean water after the treatment, filter it, and dry it to obtain the pickled alumina powder;

[0121] S 3 : Add 0.8% of the surface modifier by weight of the alumina powder to the acid-washed alumina powder, use anhydrous ethanol 3 times the weight of the alumina powder as the medium, mix in a reactor for 2 hours, filter and dry after the mixing is completed to obtain pretreated alumina powder;

[0122] S 4 : The obtained pretreated alumina powder was placed in a reactor, and 10% of the mass of the alumina powder was added with isobornyl methacrylate, and stirred for 0.5 h to obtain modified alumina powder. Then, yttrium oxide powder was added and stirred for 20 min to finally obtain a ceramic powder composite.

[0123] The particle size of the aluminum oxide powder is 8 μm, and the particle size of the yttrium oxide powder is 0.6 μm.

[0124] The pickling solution is a mixture of hydrochloric acid solution and lithium fluoride, and the mass ratio of the hydrochloric acid solution to the lithium fluoride is 25:3.

[0125] The volume concentration of the hydrochloric acid solution is 35%.

[0126] A method for preparing a photocurable ceramic slurry comprises the following steps:

[0127] B 1 : Take ceramic powder composite, dipentaerythritol hexaacrylate, photoinitiator, dispersant and polyethylene glycol respectively by weight, mix them evenly and heat to 60° C., add defoamer and stir for 0.5 h to obtain slurry premix;

[0128] B 2 : The slurry premix was transferred into the reactor, stirred for 5 hours, and discharged to obtain the light-cured ceramic slurry, wherein the rotation speed was 180 r / min.

[0129] Comparative Example 4

[0130] Different from Example 3, the polyethylene glycol has not been modified; and in the preparation of the ceramic powder composite, the alumina powder has not been acid-washed or pre-treated.

[0131] A photocurable ceramic slurry comprises the following components by weight: 70 parts of a ceramic powder compound, 25 parts of dipentaerythritol hexaacrylate, 0.3 parts of a photoinitiator, 0.5 parts of a dispersant, 1.2 parts of a defoamer and 3.0 parts of polyethylene glycol.

[0132] The method for preparing a ceramic powder composite comprises the following steps:

[0133] S 1 : Weigh alumina powder and yttrium oxide powder, wherein the mass ratio of alumina powder to yttrium oxide powder is 25:3;

[0134] S 2 : Alumina powder and yttrium oxide powder are placed in a reactor and mixed evenly, 10% of the mass of alumina powder isobornyl methacrylate is added, and stirred for 0.5 h to finally obtain a ceramic powder composite.

[0135] The particle size of the aluminum oxide powder is 8 μm, and the particle size of the yttrium oxide powder is 0.6 μm.

[0136] A method for preparing a photocurable ceramic slurry comprises the following steps:

[0137] B 1 : Take ceramic powder composite, dipentaerythritol hexaacrylate, photoinitiator, dispersant and polyethylene glycol respectively by weight, mix them evenly and heat to 60° C., add defoamer and stir for 0.5 h to obtain slurry premix;

[0138] B 2 : The slurry premix was transferred into the reactor, stirred for 5 hours, and discharged to obtain the light-cured ceramic slurry, wherein the rotation speed was 180 r / min.

[0139] The photocured ceramic slurry obtained in the embodiment and the comparative example is used to prepare ceramic specimens. The specific preparation process is as follows: the ceramic slurry is placed under a photocuring printer, the photocuring time is controlled to be 40s, the slice thickness is 50μm, and the ceramic specimen embryo is obtained after printing is completed. The ceramic specimen embryo is then heated to 500℃ at a heating rate of 2℃ / min, kept warm for 2h, and then heated to 1750℃ at a heating rate of 5℃ / min, kept warm for 4h, and cooled to obtain the ceramic specimen.

[0140] The viscosity and anti-settling properties of the obtained ceramic slurry and the mechanical properties of the ceramic specimens were tested respectively, and the specific data are shown in Table 1;

[0141] Table 1

[0142]

[0143] From the tensile strength, viscosity and anti-settling performance of the ceramic slurries prepared in each of Examples 1 to 3 in Table 1, it can be seen that the ceramic slurries prepared by the technical solution of the present invention have excellent mechanical properties and can be placed for a long time without deterioration, and are convenient to use.

[0144] The difference between Comparative Example 1 and Example 3 is that in the preparation of the ceramic powder composite, isobornyl methacrylate is not added in the treatment of step 4.

[0145] The tensile strength of the ceramic slurry prepared in Comparative Example 1 is less than that of the ceramic slurry prepared in Example 3, and the anti-settling performance of the ceramic slurry prepared in Example 3 is better than the anti-settling performance of the ceramic slurry prepared in Comparative Example 1.

[0146] The above indicates that isobornyl methacrylate can improve the mechanical properties of the prepared ceramic slurry and prolong the placement time of the ceramic slurry.

[0147] The difference between Comparative Example 2 and Example 3 is that the alumina powder is neither acid washed nor pretreated in the preparation of the ceramic powder composite.

[0148] The tensile strength of the ceramic slurry prepared in Comparative Example 2 is less than that of the ceramic slurry prepared in Example 3, and the anti-settling performance of the ceramic slurry prepared in Example 3 is better than that of the ceramic slurry prepared in Comparative Example 2.

[0149] The above indicates that the modification treatment of alumina powder after pickling can improve the mechanical properties of the prepared ceramic slurry and prolong the placement time of the ceramic slurry.

[0150] Comparative Example 3 is different from Example 3 in that the polyethylene glycol is not modified.

[0151] The tensile strength of the ceramic slurry prepared in Comparative Example 3 is less than the tensile strength of the ceramic slurry prepared in Example 3, and the anti-settling performance of the ceramic slurry prepared in Example 3 is better than the anti-settling performance of the ceramic slurry prepared in Comparative Example 3.

[0152] The above indicates that modification of polyethylene glycol can improve the mechanical properties of the prepared ceramic slurry and prolong the placement time of the ceramic slurry.

[0153] Comparative Example 4 is different from Example 3 in that the polyethylene glycol is not modified; and in the preparation of the ceramic powder composite, the alumina powder is neither acid-washed nor pre-treated.

[0154] The tensile strength of the ceramic slurry prepared in Comparative Example 4 is less than that of the ceramic slurry prepared in Example 3, and the anti-settling performance of the ceramic slurry prepared in Example 3 is better than that of the ceramic slurry prepared in Comparative Example 4.

[0155] Combining Comparative Examples 2 and 3, it can be seen that the modified alumina powder and the modified polyethylene glycol can synergistically improve the mechanical properties of the ceramic slurry and extend the placement time of the ceramic slurry during the preparation of the ceramic slurry, making it convenient to use and reducing resource waste.

[0156] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A photocurable ceramic slurry, characterized in that: The invention comprises the following components by weight: 65 to 75 parts of ceramic powder composite, 24 to 26 parts of dipentaerythritol hexaacrylate, 0.2 to 0.4 parts of photoinitiator, 0.4 to 0.6 parts of dispersant, 1.0 to 1.4 parts of defoamer and 2.5 to 3.5 parts of modified polyethylene glycol.

2. The photocurable ceramic slurry according to claim 1, characterized in that: The method for preparing the ceramic powder composite comprises the following steps: S1: weighing aluminum oxide powder and yttrium oxide powder, wherein the mass ratio of aluminum oxide powder to yttrium oxide powder is (20-30):3; S2: placing the alumina powder in a pickling solution 10 to 15 times the weight of the alumina powder, treating it in a water bath at 40 to 50° C. for 4 to 8 hours, washing it with clean water after the treatment, filtering it, and drying it to obtain the pickled alumina powder; S3: adding 0.6-1.0% of the surface modifier by weight of the alumina powder to the acid-washed alumina powder, using 2-5 times the weight of the alumina powder as anhydrous ethanol as a medium, mixing in a reactor for 2-3 hours, filtering and drying after the mixing is completed, to obtain pretreated alumina powder; S4: Put the obtained pretreated alumina powder into a reactor, add 8-12% of isobornyl methacrylate by weight of the alumina powder, stir for 0.5-1h to obtain modified alumina powder, then add yttrium oxide powder, stir for 20-30min, and finally obtain a ceramic powder composite.

3. The photocurable ceramic slurry according to claim 2, characterized in that: The particle size of the aluminum oxide powder is 6 to 10 μm, and the particle size of the yttrium oxide powder is 0.25 to 1 μm.

4. The photocurable ceramic slurry according to claim 2, characterized in that: The pickling solution is a mixed solution of hydrochloric acid solution and lithium fluoride, and the mass ratio of the hydrochloric acid solution to the lithium fluoride is (20-30):

3.

5. The photocurable ceramic slurry according to claim 4, characterized in that: The volume concentration of the hydrochloric acid solution is 30-40%.

6. The photocurable ceramic slurry according to claim 2, characterized in that: The surface modifier is KH560.

7. The photocurable ceramic slurry according to claim 1, characterized in that: The photoinitiator is phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide, the dispersant is BYK111, and the defoamer is polydimethylsiloxane.

8. The photocurable ceramic slurry according to claim 1, characterized in that: The preparation method of the modified polyethylene glycol comprises the following steps: A1: Add 3-5 parts of lignin by weight into a reactor, then add 6-8 parts of dimethylaminoethyl methacrylate and 60 parts of polyethylene glycol-400, start stirring, heat to 50-60°C and react for 1-1.5 hours. After the reaction is completed, an intermediate product is obtained; A2: The intermediate product is washed with water and rotary evaporated at a temperature of 80 to 85°C, a pressure of 5 to 7 hPa, and a time of 0.5 to 1 h, and then activated carbon is added for adsorption and decolorization to obtain modified polyethylene glycol.

9. A method for preparing a photocurable ceramic slurry according to any one of claims 1 to 8, characterized in that: The following steps are involved: B1: Take ceramic powder composite, dipentaerythritol hexaacrylate, photoinitiator, dispersant and modified polyethylene glycol respectively by weight, mix them evenly, heat to 50-70°C, add defoamer, stir for 0.5-1h, and obtain slurry premix; B2: Transfer the slurry premix to the reactor, stir for 4 to 6 hours, and discharge to obtain the light-cured ceramic slurry, wherein the rotation speed is 150 to 200 r / min.

Citation Information

Patent Citations

  • Method for controlling ceramic slurry curing proceeding

    CN101423397A

  • Aluminum oxide ceramic slurry for photocuring 3D printing, preparation method and aluminum oxide ceramic

    CN114075069A

  • Photocuring 3D printing alumina-based ceramic material as well as preparation method and application thereof

    CN115991595A

  • Silicon dioxide composite silicon nitride ceramic photocuring slurry, preparation and low-heat-conductivity porous ceramic preparation method

    CN118420376A

  • Method for treating organic-wastes

    KR1020100012798A