Polyurethane fluoride-free water repellent and preparation method thereof

Through the chemical reaction of raw materials such as polyphthalylphenylenediamine, sodium dichloroisocyanurate and terminal hydroxypolysiloxane, the prepared polyurethane fluorine-free water repellent maintains excellent waterproofing effect in extreme environments and long-term use. The problems of reduced waterproofing effect and insufficient oil resistance in the prior art have been solved, and excellent performance under high temperature, low temperature and ultraviolet light have been achieved.

CN119081050APending Publication Date: 2024-12-06ZHEJIANG LIANSHENG NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411444605.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing polyurethane fluorine-free water repellents have gradually decreased waterproofing effects under extreme environmental conditions or after long-term use, and their stability is poor, while lacking oil resistance.

Method used

Polyurethane fluorine-free water repellent is prepared through specific chemical reaction steps using raw materials such as polyphthalylphenylenediamine, sodium dichloroisocyanurate and terminal hydroxyl polysiloxane, including maintaining water repellent in high and low temperature environments. , and maintain excellent results under ultraviolet rays.

Benefits of technology

The prepared polyurethane fluorine-free water repellent maintains good water repellency in high and low temperature environments, and can maintain excellent waterproofing effect under long-term ultraviolet irradiation, and has certain oil-proofing effect, stability and environmental friendliness. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081050A_ABST
    Figure CN119081050A_ABST
Patent Text Reader

Abstract

The invention discloses a polyurethane fluoride-free water repellent and a preparation method thereof. The structural formula of the polyurethane fluoride-free water repellent is as follows: # imgabs0 #. The polyurethane fluoride-free water repellent has the beneficial effects that the prepared polyurethane fluoride-free water repellent has a certain oil-proof effect, can keep better water repellency after being used in high-temperature and low-temperature environments, and can also keep an excellent water repellency effect after being used under ultraviolet irradiation for a long time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water repellents, in particular to a polyurethane fluorine-free water repellent and a preparation method thereof. Background Art

[0002] With the continuous advancement of science and technology, people have higher and higher functional demands on textiles. In real life, textiles are inevitably exposed to water and oil stains during wearing or using. Therefore, water-repellent textiles have gradually entered people's lives. At present, fluorinated water repellents have shown superior performance in water-repellent finishing, but the physiological toxicity and environmental degradation of fluorinated water repellents have gradually emerged. At the same time, with the enhancement of people's safety awareness and environmental awareness, fluorine-free water repellents have become a new research topic.

[0003] As an environmentally friendly and high-performance textile auxiliary agent, polyurethane fluorine-free water repellent is widely used in the field of textile waterproof finishing. First of all, its comprehensive performance is excellent. Polyurethane fluorine-free water repellent can form a very soft film, which can improve the water-repellent performance of the finished fabric while maintaining a good feel and softness. Polyurethane fluorine-free water repellent also has good washing resistance, and can still maintain a good waterproof effect even after multiple washings; secondly, the fabrics finished with polyurethane fluorine-free water repellent have less hand scratches, which means that during daily wear and use, the fabrics are not easy to produce obvious marks due to friction, thereby keeping the fabrics clean and beautiful; in addition, some polyurethane fluorine-free water repellents can also show excellent anti-siphoning performance in the waterproof finishing of specific materials such as webbing and shoe materials, which is particularly important for application scenarios that require special waterproof performance. Moreover, polyurethane fluorine-free water repellent does not contain fluorine elements, so it will not cause pollution to the environment during use, which meets modern environmental protection requirements.

[0004] However, although polyurethane fluorine-free water repellent has good washing resistance, it has poor oil resistance, and its waterproof effect may gradually decrease under extreme environmental conditions or after long-term use, and its stability is poor.

[0005] In order to solve the existing problems, we propose a polyurethane fluorine-free water repellent. Summary of the invention

[0006] The purpose of the present invention is to provide a polyurethane fluorine-free water repellent and a preparation method thereof to solve the problems raised in the above background technology. The prepared polyurethane fluorine-free water repellent has a certain oil-proof effect, and can maintain good water repellency after being used in high and low temperature environments, and can also maintain excellent water repellency after being used under long-term ultraviolet irradiation.

[0007] To achieve the above object, the present invention provides a polyurethane fluorine-free water repellent, the structural formula of which is as follows: .

[0008] Preferably, the raw materials of the polyurethane fluorine-free water repellent include polyphenylene phthalate, sodium dichloroisocyanurate and terminal hydroxyl polysiloxane.

[0009] The present invention also provides a method for preparing the above-mentioned polyurethane fluorine-free water repellent, comprising the following steps: S1, adding polyphenylene phthalamide to an aqueous solution of sodium dichloroisocyanurate, adding hydrochloric acid and heating after the reaction is completed, and then purifying to obtain an intermediate 1; S2, putting intermediate 1 into concentrated sulfuric acid to obtain intermediate 2; S3, putting the intermediate 2 into concentrated nitric acid, and obtaining the intermediate 3 after the reaction is completed; S4, putting the intermediate 3 into a sodium hydroxide solution, and after the reaction is completed, washing and drying to obtain the intermediate 4; S5, preheating the intermediate 4, and passing it into COCl2, and maintaining a closed space, and after the reaction is completed, the intermediate 5 is obtained; S6, dissolving the intermediate 5 in ethanol, adding a catalyst, and after the reaction is completed, filtering to obtain the intermediate 6; S7, dissolving the intermediate product 6 in a solvent, adding terminal hydroxyl polysiloxane, adding a catalyst, and obtaining a polyurethane fluorine-free water repellent after the reaction is completed.

[0010] Preferably, in step S1, the mass ratio of polyphenylene phthalate to sodium dichloroisocyanurate aqueous solution is 1-2 parts: 150-200 parts, and the concentration of sodium dichloroisocyanurate aqueous solution is 30-80%; the specific operation of step S1 is: polyphenylene phthalate is added to the sodium dichloroisocyanurate aqueous solution, stirred at a speed of 1000-4000r / min for 2-8 min, and heated at 100-120°C for 1-2h after adding hydrochloric acid solution, and the concentration of hydrochloric acid is 40-60%.

[0011] Preferably, the reaction conditions in step S3 are a temperature of 60-80° C., a reaction time of 0.5-2 h, and stirring is maintained during the reaction at a stirring rate of 50-200 r / min.

[0012] Preferably, the mass fraction of the sodium hydroxide solution in step S4 is 30-60%, stirring is performed during the reaction, the stirring rate is 100-200 r / min, and the reaction time is 0.5-24 h.

[0013] Preferably, the reaction conditions in step S5 are as follows: the preheating temperature of the intermediate 4 is 120-180° C., the reaction temperature is 150-250° C., and the reaction time is 0.5-3 h.

[0014] Preferably, in step S6, the catalyst is triethylamine, trimethylamine, pyridine, the reaction temperature is 60-100° C., the reaction time is 1-5 h, and the pressure is 5-19 MPa.

[0015] Preferably, in step S7, the solvent is dimethylacetamide, N-methylpyrrolidone or hexamethylphosphoramide, the catalyst is bis(dimethylaminohexyl) ether or triethylenediamine, and the reaction conditions are a temperature of 20-60° C. and a reaction time of 1-48 h.

[0016] The advantages and positive effects of the polyurethane fluorine-free water repellent and the preparation method thereof described in the present invention are: 1. The polyurethane fluorine-free water repellent prepared by the present invention does not contain fluorine element, will not cause pollution to the environment during use, and meets modern environmental protection requirements. At the same time, its waterproof effect and stability are still excellent under extreme environmental conditions or after long-term use.

[0017] 2. The polyurethane fluorine-free water repellent prepared by the present invention has a certain oil-proof effect, and can maintain good water repellency after being used in high and low temperature environments, and can also maintain excellent water repellency after being used under long-term ultraviolet irradiation.

[0018] The technical solution of the present invention is preferably described in detail below through embodiments. DETAILED DESCRIPTION

[0019] The technical solution of the present invention is further illustrated by the following examples.

[0020] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.

[0021] Unless otherwise defined, the instruments, equipment and reagents used in the present invention are all commercially available.

[0022] Example 1 S1: 10 parts of polyphenylene phthalamide were added to 1500 parts of 30% sodium dichloroisocyanurate aqueous solution, stirred at 1000 r / min for 2 min, 1 part of 40% hydrochloric acid was added and heated at 100°C for 1 h to purify the intermediate 1; S2: 10 parts of intermediate 1 are added into concentrated sulfuric acid and filtered to obtain intermediate 2; S3: 10 portions of the intermediate product 2 were added to concentrated nitric acid. The process conditions were as follows: the reaction was carried out at a temperature of 60°C for 0.5 h. During the reaction, the stirring rate was maintained at 50 r / min. After the reaction was completed, the intermediate product 3 was obtained by suction filtration. S4: 10 portions of intermediate 3 are added to a sodium hydroxide solution with a mass fraction of 30%, the stirring rate is 100 r / min, the reaction time is 0.5 h, and after the reaction is completed, the intermediate 4 is washed and dried; S5: preheat 10 portions of intermediate 4 at 120°C, and introduce COCl2 in a closed space. The process conditions are to react at a temperature of 150°C for 0.5h. After the reaction is completed, intermediate 5 is obtained. S6: Dissolve 10 parts of intermediate 5 in ethanol and add 0.2 parts of catalyst triethylamine. The process conditions are to react at a temperature of 60°C and a pressure of 5 MPa for 1 hour. After the reaction is completed, filter and obtain intermediate 6.

[0023] S7: Dissolve 2 parts of intermediate 6 in 5 parts of dimethylacetamide, add 10 parts of diphenylmethane diisocyanate and 150 parts of terminal hydroxyl polysiloxane, add 0.1 part of bis(dimethylaminohexyl) ether. The process conditions are to react at a temperature of 20-60°C for 1-48h. After the reaction is completed, a polyurethane fluorine-free water repellent is obtained.

[0024] Example 2 S1: 20 parts of polyphenylene phthalamide were added to 2000 parts of 80% sodium dichloroisocyanurate aqueous solution, stirred at 4000 r / min for 8 min, 5 parts of 60% hydrochloric acid were added and heated at 120°C for 2 h to purify the intermediate 1; S2: put 20 parts of intermediate 1 into concentrated sulfuric acid and filter to obtain intermediate 2; S3: 20 parts of the intermediate product 2 are added to concentrated nitric acid. The process conditions are as follows: the reaction is carried out at a temperature of 80°C for 2 hours. During the reaction, the stirring rate is maintained at 200 r / min. After the reaction is completed, the intermediate product 3 is obtained by suction filtration. S4: 20 parts of intermediate 3 are added to a sodium hydroxide solution with a mass fraction of 60%, the stirring rate is 200r / min, the reaction time is 24h, and after the reaction is completed, the intermediate 4 is washed and dried; S5: preheat 20 portions of intermediate 4 at 180°C, and introduce COCl2 in a closed space. The process conditions are to react at a temperature of 250°C for 3 hours. After the reaction is completed, intermediate 5 is obtained. S6: Dissolve 20 parts of intermediate 5 in ethanol and add 1 part of trimethylamine. The process conditions are to react at a temperature of 100°C and a pressure of 19 MPa for 5 hours. After the reaction is completed, filter and obtain intermediate 6.

[0025] S7: Dissolve 3 parts of intermediate 6 in 10 parts of N-methylpyrrolidone, add 10-20 parts of diphenylmethane diisocyanate and 250 parts of terminal hydroxyl polysiloxane, add 0.5 parts of triethylenediamine, and react at 60°C for 1-48h. After the reaction is completed, a polyurethane fluorine-free water repellent is obtained.

[0026] Example 3 S1: 15 parts of polyphenylene phthalamide were added to 1700 parts of 60% sodium dichloroisocyanurate aqueous solution, stirred at 3000 r / min for 5 min, 3 parts of 50% hydrochloric acid were added and heated at 110°C for 1.5 h to purify the intermediate 1; S2: 15 parts of intermediate 1 are added into concentrated sulfuric acid and filtered to obtain intermediate 2; S3: 15 portions of intermediate 2 were added to concentrated nitric acid. The process conditions were as follows: the reaction was carried out at a temperature of 70°C for 1.5 hours. During the reaction, the stirring rate was maintained at 100 r / min. After the reaction was completed, intermediate 3 was obtained by suction filtration. S4: 15 parts of intermediate 3 are added into a sodium hydroxide solution with a mass fraction of 50%, the stirring rate is 120r / min, the reaction time is 12h, and after the reaction is completed, the intermediate 4 is washed and dried; S5: preheat 15 portions of intermediate 4 at 160°C, and introduce into COCl2, and keep in a closed space. The process condition is to react at a temperature of 200°C for 1 hour. After the reaction is completed, intermediate 5 is obtained; S6: 15 parts of intermediate 5 were dissolved in ethanol, and 0.5 parts of pyridine were added. The process conditions were 70°C and 10 MPa for 3 hours. After the reaction was completed, intermediate 6 was obtained by filtration.

[0027] S7: Dissolve 2.5 parts of intermediate 6 in 7 parts of hexamethylphosphoramide, add 15 parts of diphenylmethane diisocyanate and 200 parts of terminal hydroxyl polysiloxane, add 0.4 parts of triethylenediamine, and react at 50°C for 2 hours. After the reaction is completed, a polyurethane fluorine-free water repellent is obtained.

[0028] Comparative Example 1 S1: 15 parts of polyphenylene phthalamide were added to 1700 parts of 60% hypochlorous acid aqueous solution, stirred at a speed of 3000 r / min for 5 min, and purified to obtain intermediate 1; S2: 15 parts of intermediate 1 are added into concentrated sulfuric acid and filtered to obtain intermediate 2; S3: 15 portions of intermediate 2 were added to concentrated nitric acid. The process conditions were as follows: the reaction was carried out at a temperature of 70°C for 1.5 hours. During the reaction, the stirring rate was maintained at 100 r / min. After the reaction was completed, intermediate 3 was obtained by suction filtration. S4: 15 parts of intermediate 3 are added into a sodium hydroxide solution with a mass fraction of 50%, the stirring rate is 120r / min, the reaction time is 12h, and after the reaction is completed, the intermediate 4 is washed and dried; S5: preheat 15 portions of intermediate 4 at 160°C, and introduce into COCl2, and keep in a closed space. The process condition is to react at a temperature of 200°C for 1 hour. After the reaction is completed, intermediate 5 is obtained; S6: 15 parts of intermediate 5 were dissolved in ethanol, and 0.5 parts of pyridine were added. The process conditions were 70°C and 10 MPa for 3 hours. After the reaction was completed, intermediate 6 was obtained by filtration.

[0029] S7: Dissolve 2.5 parts of intermediate 6 in 7 parts of hexamethylphosphoramide, add 15 parts of diphenylmethane diisocyanate and 200 parts of terminal hydroxyl polysiloxane, add 0.4 parts of triethylenediamine, and react at 50°C for 2 hours. After the reaction is completed, a polyurethane fluorine-free water repellent is obtained.

[0030] Comparative Example 2 S1: 15 parts of polyphenylene phthalamide were added to 1700 parts of 60% sodium dichloroisocyanurate aqueous solution, stirred at 3000 r / min for 5 min, 3 parts of 50% hydrochloric acid were added and heated at 110°C for 1.5 h to purify the intermediate 1; S2: preheat 15 parts of intermediate 1 at 160°C, and pass into COCl2 in a closed space. The process condition is to react at a temperature of 200°C for 1 hour. After the reaction is completed, intermediate 2 is obtained. S3: 15 parts of intermediate 2 were dissolved in ethanol, and 0.5 parts of pyridine were added. The process conditions were 70°C and 10 MPa for 3 hours. After the reaction was completed, intermediate 3 was obtained by filtration.

[0031] S4: Dissolve 2.5 parts of intermediate 3 in 7 parts of hexamethylphosphoramide, add 15 parts of diphenylmethane diisocyanate and 200 parts of terminal hydroxyl polysiloxane, add 0.4 parts of triethylenediamine, and react at 50°C for 2 hours. After the reaction is completed, a polyurethane fluorine-free water repellent is obtained.

[0032] Comparative Example 3 0.4 parts of triethylenediamine were added to 15 parts of diphenylmethane diisocyanate and 200 parts of terminal hydroxyl polysiloxane. The process conditions were to react at a temperature of 50°C for 2 hours. After the reaction was completed, a polyurethane fluorine-free water repellent was obtained.

[0033] Performance Testing The fabrics treated with the polyurethane fluorine-free water repellent prepared in Examples 1-3 and Comparative Examples 1-3 were tested for contact angle, oil repellency, low temperature resistance, high temperature resistance and durability.

[0034] Oil repellency test: Drop peanut oil on the fabric, test the contact angle of each fabric and calculate the average value.

[0035] Low temperature resistance: Place the fabric in a -40℃ freezer for 48 hours, take it out and return it to room temperature, test the contact angle of each fabric and calculate the average value.

[0036] High temperature resistance: Place the fabric in a 40°C freezer for 48 hours, take it out and return it to room temperature, then test the contact angle of each fabric and calculate the average value.

[0037] Durability test: After placing the fabric outdoors for one year, test the contact angle of each fabric and calculate the average value.

[0038] The test results are shown in Table 1: Table 1 Test results

[0039] By comparing Examples 1-3 and Comparative Example 3, it can be seen that the conventional contact angle is about 7% higher than that of Comparative Example 3, the contact angle tested after oil drop in Examples 1-3 is about 25% higher than that of Comparative Example 3, the contact angle after low temperature treatment is about 15% higher, the contact angle after high temperature treatment is about 25% higher, and the contact angle after durability test treatment is about 11% higher.

[0040] By comparing Examples 1-3 with Comparative Example 1, it can be seen that the conventional contact angle is increased by about 6% compared with Comparative Example 1, the contact angle tested after oil dropping of Examples 1-3 is increased by about 20% compared with Comparative Example 1, the contact angle after low-temperature treatment is increased by about 6%, the contact angle after high-temperature treatment is increased by about 5%, and the contact angle after durability test treatment is increased by about 5%.

[0041] By comparing Examples 1-3 with Comparative Example 2, it can be seen that the conventional contact angle is increased by about 6% compared with Comparative Example 2, the contact angle tested after oil dropping of Examples 1-3 is increased by about 20% compared with Comparative Example 2, the contact angle after low-temperature treatment is increased by about 8%, the contact angle after high-temperature treatment is increased by about 10%, and the contact angle after durability test treatment is increased by about 7%.

[0042] The comprehensive conclusion is that the polyurethane fluorine-free water repellent has a certain oil-proof effect, and can maintain good water repellency after being used in high and low temperature environments, and can also maintain excellent water repellency after being used under long-term ultraviolet radiation.

[0043] Therefore, the present invention adopts the above-mentioned polyurethane fluorine-free water repellent and its preparation method. The prepared polyurethane fluorine-free water repellent has a certain oil-proof effect, and can maintain good water repellency after being used in high and low temperature environments, and can also maintain excellent water repellency after being used under long-term ultraviolet irradiation.

[0044] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A polyurethane fluorine-free water repellent, characterized in that: The structural formula of the polyurethane fluorine-free water repellent is as follows: 。 2. A polyurethane fluorine-free water repellent according to claim 1, characterized in that: The raw materials of polyurethane fluorine-free water repellent include polyphenylene phthalate, sodium dichloroisocyanurate and terminal hydroxyl polysiloxane.

3. The method for preparing a polyurethane fluorine-free water repellent according to claim 1, characterized in that: The following steps are involved: S1, adding polyphenylene phthalamide to an aqueous solution of sodium dichloroisocyanurate, adding hydrochloric acid and heating after the reaction is completed, and then purifying to obtain an intermediate 1; S2, putting intermediate 1 into concentrated sulfuric acid to obtain intermediate 2; S3, putting the intermediate 2 into concentrated nitric acid, and obtaining the intermediate 3 after the reaction is completed; S4, putting the intermediate 3 into a sodium hydroxide solution, and after the reaction is completed, washing and drying to obtain the intermediate 4; S5, preheating the intermediate 4, and passing it into COCl2, and maintaining a closed space, and after the reaction is completed, the intermediate 5 is obtained; S6, dissolving the intermediate 5 in ethanol, adding a catalyst, and after the reaction is completed, filtering to obtain the intermediate 6; S7, dissolving the intermediate product 6 in a solvent, adding terminal hydroxyl polysiloxane, adding a catalyst, and obtaining a polyurethane fluorine-free water repellent after the reaction is completed.

4. The preparation method according to claim 3, characterized in that: In step S1, the mass ratio of polyphenylene phthalate to sodium dichloroisocyanurate aqueous solution is 1-2 parts: 150-200 parts, and the concentration of sodium dichloroisocyanurate aqueous solution is 30-80%. The specific operation of step S1 is: polyphenylene phthalate is added to the sodium dichloroisocyanurate aqueous solution, stirred at a speed of 1000-4000r / min for 2-8 minutes, and heated at 100-120°C for 1-2 hours after adding hydrochloric acid solution, and the concentration of hydrochloric acid is 40-60%.

5. The preparation method according to claim 3, characterized in that: The reaction conditions in step S3 are a temperature of 60-80° C., a reaction time of 0.5-2 h, and stirring is maintained during the reaction at a stirring rate of 50-200 r / min.

6. The preparation method according to claim 3, characterized in that: In step S4, the mass fraction of the sodium hydroxide solution is 30-60%, stirring is performed during the reaction, the stirring rate is 100-200 r / min, and the reaction time is 0.5-24h.

7. The preparation method according to claim 3, characterized in that: The reaction conditions in step S5 are as follows: the preheating temperature of the intermediate 4 is 120-180° C., the reaction temperature is 150-250° C., and the reaction time is 0.5-3 h.

8. The preparation method according to claim 3, characterized in that: In step S6, the catalyst is triethylamine, trimethylamine, and pyridine, the reaction temperature is 60-100° C., the reaction time is 1-5 h, and the pressure is 5-19 MPa.

9. The preparation method according to claim 3, characterized in that: In step S7, the solvent is dimethylacetamide, N-methylpyrrolidone or hexamethylphosphoramide, the catalyst is bis(dimethylaminohexyl) ether or triethylenediamine, the reaction conditions are a temperature of 20-60° C., and a reaction time of 1-48 h.