High-water-resistance waterborne polyurethane resin film as well as preparation method and application thereof
By using combined materials such as macromolecular polyols and polyisocyanates in the aqueous polyurethane resin film, and using UV catalytic chain extension reaction of N,N-dimethacrylate, the problem of insufficient water resistance of the aqueous polyurethane resin film is solved, which significantly It improves its performance in water environment and is suitable for leather manufacturing and other fields.
Patent Information
- Application Number
- CN202411344753.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-12-06
AI Technical Summary
The existing water-based polyurethane resin films are insufficient in water environments, which affects their application quality in leather manufacturing and other fields.
Using a combination of macromolecular polyols, polyisocyanates, hydrophilic chain extenders, small-molecular alcohol chain extenders, amine chain extenders, catalysts, salt forming agents and initiators, etc., the high-quality can be formed through specific reaction steps and conditions. Water-resistant polyurethane resin film uses N,N-dimethacrylate as a salt forming agent to perform chain extension reaction under UV catalysis to improve the water resistance of the resin.
It significantly improves the water resistance of the water-based polyurethane resin film, so that it maintains good physical and chemical properties in humid environments, and is suitable for leather manufacturing and other fields.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyurethane resins, and in particular to a highly water-resistant water-based polyurethane resin film and a preparation method and application thereof. Background Art
[0002] Waterborne polyurethane is being used in more and more fields, especially in leather manufacturing, due to its safety and environmental protection characteristics. The water resistance index of waterborne polyurethane is crucial. Water resistance usually refers to the ability of a material to maintain its physical and chemical properties in a water environment. For waterborne polyurethane resins, water resistance is mainly reflected in the stability of its coating or film layer in water. The most important point is the impact on mechanical properties in an aqueous environment. The better the water resistance of waterborne polyurethane resins, the better its quality of use.
[0003] Based on this, the present invention is committed to providing a highly water-resistant water-based polyurethane resin film and a preparation method and use thereof. Summary of the invention
[0004] The object of the present invention is to provide a highly water-resistant water-based polyurethane resin film and a preparation method and use thereof, so as to solve the following technical problems:
[0005] How to improve the water resistance of waterborne polyurethane resin film.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] In a first aspect, the present invention discloses a highly water-resistant water-based polyurethane resin film, comprising the following raw materials in parts by weight:
[0008] 150-200 parts of macromolecular polyol, 40-70 parts of polyisocyanate, 5-12 parts of hydrophilic chain extender, 1-7 parts of small molecule alcohol chain extender, 2-12 parts of amine chain extender, 0.1-1 parts of catalyst, 3-8 parts of salt former, 2-12 parts of initiator;
[0009] Preferably, the macromolecular polyol is 160-180 parts, the polyisocyanate is 45-60 parts, the hydrophilic chain extender is 6-9 parts, the small molecule alcohol chain extender is 1-5 parts, the amine chain extender is 2-5 parts, the catalyst is 0.1-0.5 parts, the salt former is 2-6 parts, and the initiator is 3-7 parts.
[0010] Further, the macromolecular polyol includes any one or a mixture of any two or more of polyester polyol, polycarbonate polyol, polytetramethylene polyol, polyoxypropylene polyol, polysiloxane polyol and bio-based polyol;
[0011] Preferably, the molecular weight of the macropolyol is 1000-3000.
[0012] Further, the polyisocyanate includes any one of toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, p-phenylene diisocyanate, 1,4-cyclohexane diisocyanate, cyclohexane dimethylene diisocyanate, tetramethyl meta-xylylene diisocyanate, and methylcyclohexyl diisocyanate, or a mixture of any two or more thereof;
[0013] Further, the hydrophilic chain extender is any one of dimethylol propionic acid and dimethylol butyric acid or a mixture of the two;
[0014] Preferably, the hydrophilic chain extender is dimethylolpropionic acid.
[0015] Furthermore, the small molecule alcohol chain extender includes any one of ethylene glycol, 1,4-butanediol, 1,3-butanediol, 1,2-propylene glycol, diethylene glycol, neopentyl glycol, methyl propanediol, 1,6-hexanediol, 1,3-propylene glycol, diethyl pentanediol, trimethyl pentanediol, ethyl hexanediol, dodecanediol and cyclohexanediol, or a mixture of any two or more thereof.
[0016] Furthermore, the amine chain extender includes any one or a mixture of any two or more of hexamethylenediamine, isophoronediamine, diaminocyclohexylmethane, trimethylhexamethylenediamine, 1,3-cyclohexanedimethylamine and 1,4-cyclohexanedimethylamine.
[0017] Furthermore, the catalyst is any one of an organic bismuth catalyst and a tertiary amine catalyst, or a mixture of both;
[0018] Preferably, the catalyst is an organic bismuth catalyst.
[0019] Furthermore, the salt-forming agent is N,N-dimethylpropyleneamine.
[0020] Furthermore, the initiator includes any one or a mixture of any two or more of phenylacetone, 4-chlorobenzophenone, ethyl 2,4,6-trimethylbenzoylphosphonate, dimethyl benzoate, methyl o-benzoylbenzoate, a mixture of benzoylformic acid esters, and 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide.
[0021] In a second aspect, the present invention discloses a method for producing a highly water-resistant aqueous polyurethane resin film as described above, comprising the following steps:
[0022] The macromolecular polyol and polyisocyanate are reacted at 85-95°C for 2h; then a hydrophilic chain extender and a small molecule alcohol chain extender are added and reacted at 80-85°C for 2h; a catalyst is added and reacted at 60-70°C for 3h, and after cooling to 8-15°C, N,N-dimethylpropyleneamine is added for neutralization; ice water is added for emulsification, and then an amine chain extender is added, and finally, the solvent is removed by vacuum distillation, and then an initiator is added and stirred evenly to obtain a waterborne polyurethane resin. After the waterborne polyurethane resin is spread as a film, UV irradiation is performed for 3min, and after drying and solidification, a highly water-resistant waterborne polyurethane resin film is obtained.
[0023] Furthermore, methyl methyl carbamate is added at the same time as the hydrophilic chain extender; the main function of methyl methyl carbamate is to dissolve the hydrophilic chain extender, and the addition amount thereof is 2%-3% of the emulsion.
[0024] Furthermore, before adding the salt-forming agent, a proper amount of acetone is added to reduce the viscosity. The amount of acetone can be increased appropriately according to the viscosity of the system, and the increased acetone will be removed after the reaction is completed.
[0025] In a third aspect, the present invention also discloses a use of the highly water-resistant aqueous polyurethane resin film as described above for preparing leather.
[0026] Beneficial effects of the present invention:
[0027] The highly water-resistant water-based polyurethane resin film of the present invention adopts N,N-dimethylpropyleneamine as a salt-forming agent. N,N-dimethylpropyleneamine undergoes a chain extension reaction under UV catalysis, and after the reaction, it separates from the main chain to form a long single chain, so that the resin loses its hydrophilicity, thereby improving the water resistance of the main chain of the water-based polyurethane without affecting the structure of the main chain of the water-based polyurethane. Therefore, the water resistance of the water-based polyurethane resin film can be greatly improved, so that the water-based polyurethane resin film can maintain good performance in a humid environment, and can be widely used in the field of leather manufacturing. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.
[0030] Example 1
[0031] Preparation of waterborne polyurethane resin film:
[0032] 180g of polytetrahydrofuran polyol (molecular weight 2000) was dehydrated at 105°C for 1h, then cooled to 50°C, 46g of toluene diisocyanate was added, the temperature was raised to 85°C and kept for reaction for 2h, and then the -NCO content was measured. When the theoretical value was reached, the temperature was lowered to 60°C, and then 7g of dihydroxymethylpropionic acid, 2g of 1,4-butanediol and 10g of methyl methylcarbamate were added and reacted at 80°C for 2h, and then 0.3g of organic bismuth catalyst was added and reacted at 70°C for 3h. After the reaction was completed, the -NCO content was measured, and then the temperature was lowered to 10 ℃, 100g acetone was added to reduce the viscosity and 4.44g N,N-dimethylpropyleneamine was added to neutralize for 3min, deionized water was added under high-speed shearing, dispersed for 1min, 3.1g ethylenediamine was slowly added dropwise and stirred for 3min; after the emulsion was allowed to stand for 4h, acetone in the system was removed by vacuum distillation, and finally 4.9g phenylacetone was added and stirred evenly to obtain a waterborne polyurethane resin sample 1. The solid content of sample 1 was determined to be 40.1%; after sample 1 was spread on a film, it was irradiated with UV for 3 minutes and then dried and solidified to obtain a waterborne polyurethane film.
[0033] Example 2
[0034] 170g of propylene oxide polyol (molecular weight 2000) was dehydrated at 105°C for 1h, then cooled to 50°C, 50g of toluene diisocyanate was added, the temperature was raised to 85°C and kept for reaction for 2h, and then the -NCO content was measured. When the theoretical value was reached, the temperature was lowered to 60°C, and then 6.6g of dihydroxymethylpropionic acid, 4.1g of 1,4-butanediol and 10g of methyl methylcarbamate were added and reacted at 80°C for 2h, and then 0.3g of organic bismuth catalyst was added and reacted at 70°C for 3h. After the reaction was completed, the -NCO content was measured, and then the temperature was lowered to At 10°C, 100g of acetone was added to reduce the viscosity, and 4.19g of N,N-dimethylpropyleneamine was added to neutralize for 3min, and then deionized water was added under high-speed shearing. After dispersion for 1min, 3.4g of ethylenediamine was slowly added dropwise and stirred for 3min. After the emulsion was allowed to stand for 4h, acetone was removed from the system by vacuum distillation, and finally 4.9g of phenylacetone was added and stirred evenly to obtain a waterborne polyurethane resin sample 2. The solid content of sample 2 was determined to be 41%; after spreading the sample 2, UV irradiation was performed for 3 minutes, and then drying and solidification was performed to obtain a waterborne polyurethane film.
[0035] Example 3
[0036] 100g of polytetrahydrofuran polyol (molecular weight 2000) and 80g of polyoctyl adipate (molecular weight 2000) polyol were dehydrated at 105°C for 1h, then cooled to 50°C, 45g of toluene diisocyanate was added, the temperature was raised to 85°C and kept for reaction for 2h, and then the -NCO content was measured. When the theoretical value was reached, the temperature was lowered to 60°C, and then 7.0g of dihydroxymethylpropionic acid, 1.0g of methyl propanediol and 10g of methyl methyl carbamate were added and reacted at 80°C for 2h, and then 0.3g of organic bismuth catalyst was added and reacted at 70°C for 3h. The -NCO content was measured after the reaction was completed. , then cooled to 10°C, 100g of acetone was added to reduce the viscosity, and 4.44g of N,N-dimethylpropyleneamine was added to neutralize for 3 minutes, and deionized water was added under high-speed shearing. After dispersion for 1 minute, 5.0g of 1,3-cyclohexanedimethylamine was slowly added dropwise and stirred for 3 minutes; after the emulsion was allowed to stand for 4 hours, acetone in the system was removed by vacuum distillation, and finally 5.2g of methyl o-benzoylbenzoate was added and stirred evenly to obtain a waterborne polyurethane resin sample 3. The solid content of sample 3 was determined to be 39.8%; after sample 3 was laid as a film, it was irradiated with UV for 3 minutes, and then dried and solidified to obtain a waterborne polyurethane film.
[0037] Example 4
[0038] 120g of polyoxypropylene polyol (molecular weight 2000) and 60g of polytetramethylene glycol (molecular weight 2000) were dehydrated at 105°C for 1h, then cooled to 50°C, 50g of isophorone diisocyanate was added, the temperature was raised to 90°C and kept for reaction for 2h, and then the -NCO content was determined. When the theoretical value was reached, the temperature was lowered to 70°C, and then 6.0g of dimethylol propionic acid, 3.18g of 1,4-butanediol and 10g of methyl methylcarbamate were added and reacted at 80°C for 2h, and then 0.3g of organic bismuth catalyst was added and reacted at 70°C for 3h. After the reaction was completed, the -NC content was determined. O content, then cooled to 10°C, 80g acetone was added to reduce the viscosity, 3.81g N,N-dimethylpropyleneamine was added to neutralize for 3min, deionized water was added under high-speed shearing, dispersed for 1min, 5.64g 1,4-cyclohexanedimethylamine was slowly added dropwise, and stirred for 3min; after the emulsion was allowed to stand for 4h, it was distilled under reduced pressure to remove the acetone in the system, and finally 5.2g phenylacetone was added and stirred evenly to obtain a waterborne polyurethane resin sample 4. The solid content of sample 4 was measured to be 40.3%; after sample 4 was laid as a film, it was irradiated with UV for 3 minutes, and then dried and solidified to obtain a waterborne polyurethane film.
[0039] Example 5
[0040] 80g of polyoxypropylene polyol (molecular weight 2000) and 100g of polyoxypropylene polyol (molecular weight 2000) were dehydrated at 105°C for 1h, then cooled to 50°C, 54g of isophorone diisocyanate was added, the temperature was raised to 90°C and kept for reaction for 2h, and then the -NCO content was measured. When the theoretical value was reached, the temperature was lowered to 70°C, and then 5.8g of dihydroxymethylpropionic acid, 3.8g of methyl propanediol and 10g of methyl methyl carbamate were added and reacted at 85°C for 2h, and then 0.3g of organic bismuth catalyst was added and reacted at 70°C for 3h. After the reaction was completed, the -NCO content was measured. content, then cooled to 10°C, 80g of acetone was added to reduce the viscosity, 3.68g of N,N-dimethylpropyleneamine was added to neutralize for 3min, deionized water was added under high-speed shearing, dispersed for 1min, 2.62g of 1,4-cyclohexanedimethylamine was slowly added dropwise, and stirred for 3min; after the emulsion was allowed to stand for 4h, it was distilled under reduced pressure to remove the acetone in the system, and finally 6.2g of benzoin dimethyl ether was added and stirred evenly to obtain a waterborne polyurethane resin sample 5. It was determined that the solid content of sample 5 was 38%; after spreading the sample 5, UV irradiation was performed for 3 minutes, and then drying and solidification was performed to obtain a waterborne polyurethane film.
[0041] Comparative Example 1
[0042] After the waterborne polyurethane resin sample 5 prepared in Example 5 was laid as a film, it was directly dried and solidified without UV irradiation to obtain a waterborne polyurethane film.
[0043] The waterborne polyurethane films prepared in Examples 1-5 and Comparative Example 1 were respectively subjected to performance tests, and the test method was as follows: referring to GB / T 1040-92 "Test Method for Tensile Properties of Plastics" to test the tensile strength and elongation at break of the obtained waterborne polyurethane films, and after the test, the waterborne polyurethane films were soaked in 25°C water for 1 hour and then retested to obtain the corresponding tensile strength and elongation at break results; the test results are listed in Table 1, which is as follows:
[0044] Table 1
[0045]
[0046] By analyzing the data in Table 1, it can be seen that the change rates of tensile strength and elongation at break of the waterborne polyurethane films prepared in Examples 1-5 before and after immersion in water are maintained within a stable range, and the water resistance is good. However, compared with Comparative Example 5, the change rate of Comparative Example 1 is greatly improved, which indicates that the performance of the waterborne polyurethane film prepared in Comparative Example 1 is greatly reduced after immersion in water, and its water resistance is significantly worse.
[0047] In summary, the waterborne polyurethane film prepared by the preparation method of the present invention has stronger water resistance and can improve the tensile strength and elongation of the resin in a humid environment.
[0048] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A highly water-resistant water-based polyurethane resin film, characterized in that: The invention comprises the following raw materials in parts by weight: 150-200 parts of macromolecular polyol, 40-70 parts of polyisocyanate, 5-12 parts of hydrophilic chain extender, 1-7 parts of small molecule alcohol chain extender, 2-12 parts of amine chain extender, 0.1-1 parts of catalyst, 3-8 parts of salt former, 2-12 parts of initiator; Wherein, the salt-forming agent is N,N-dimethylpropyleneamine.
2. The highly water-resistant water-based polyurethane resin film according to claim 1, characterized in that: The macromolecular polyol includes any one or a mixture of any two or more of polyester polyol, polycarbonate polyol, polytetramethylene polyol, polyoxypropylene polyol, polysiloxane polyol and bio-based polyol.
3. The highly water-resistant water-based polyurethane resin film according to claim 1, characterized in that: The polyisocyanate includes any one of toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, p-phenylene diisocyanate, 1,4-cyclohexane diisocyanate, cyclohexane dimethylene diisocyanate, tetramethyl meta-xylylene diisocyanate, and methylcyclohexyl diisocyanate, or a mixture of any two or more thereof.
4. The highly water-resistant water-based polyurethane resin film according to claim 1, characterized in that: The hydrophilic chain extender is any one of dimethylol propionic acid and dimethylol butyric acid or a mixture of the two.
5. The highly water-resistant water-based polyurethane resin film according to claim 1, characterized in that: The small molecule alcohol chain extender includes any one of ethylene glycol, 1,4-butanediol, 1,3-butanediol, 1,2-propylene glycol, diethylene glycol, neopentyl glycol, methyl propylene glycol, 1,6-hexanediol, 1,3-propylene glycol, diethyl pentanediol, trimethyl pentanediol, ethyl hexanediol, dodecanediol and cyclohexanediol, or a mixture of any two or more thereof.
6. The highly water-resistant water-based polyurethane resin film according to claim 1, characterized in that: The amine chain extender includes any one or a mixture of any two or more of hexamethylenediamine, isophoronediamine, diaminocyclohexylmethane, trimethylhexamethylenediamine, 1,3-cyclohexanedimethylamine and 1,4-cyclohexanedimethylamine.
7. The highly water-resistant water-based polyurethane resin film according to claim 1, characterized in that: The catalyst is any one of an organic bismuth catalyst and a tertiary amine catalyst or a mixture of the two.
8. The highly water-resistant water-based polyurethane resin film according to claim 1, characterized in that: The initiator includes any one or a mixture of any two or more of phenylacetone, 4-chlorobenzophenone, ethyl 2,4,6-trimethylbenzoylphosphonate, benzoin dimethyl ether, methyl o-benzoylbenzoate, a mixture of benzoyl formate esters, and 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide.
9. A method for producing a highly water-resistant water-based polyurethane resin film as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: The macromolecular polyol and polyisocyanate are reacted at 85-95°C for 2h; then a hydrophilic chain extender and a small molecule alcohol chain extender are added and reacted at 80-85°C for 2h; a catalyst is added and reacted at 60-70°C for 3h, and after cooling to 8-15°C, N,N-dimethylpropyleneamine is added for neutralization; ice water is added for emulsification, and then an amine chain extender is added, and finally, the solvent is removed by vacuum distillation, and then an initiator is added and stirred evenly to obtain a waterborne polyurethane resin. After the waterborne polyurethane resin is spread as a film, UV irradiation is performed for 3min, and after drying and solidification, a highly water-resistant waterborne polyurethane resin film is obtained.
10. Use of a highly water-resistant water-based polyurethane resin film as claimed in any one of claims 1 to 8, characterized in that: Used in the preparation of leather.