Photocuring 3D printing UV resin based on lactic acid, and preparation method and application thereof
The lactic acid-based UV resin for 3D printing addresses the viscosity challenge by increasing diluent monomer content, achieving fast curing, good toughness, and improved mechanical and chemical resistance, facilitating complex shape printing with enhanced adhesion and flexibility.
Patent Information
- Application Number
- CN202411432553.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-10-14
AI Technical Summary
Existing UV light-curing resins for 3D printing have high viscosity, limiting the amount of diluent monomer that can be added, which affects the material's fluidity, coating properties, and mechanical properties such as strength and adhesion, making it difficult to construct complex shapes and increasing production costs.
A UV resin based on lactic acid is prepared by reacting lactic acid, bisphenol A epoxy resin, and acrylic acid, with a specific molar ratio, using p-hydroxyanisole as an inhibitor and triphenylphosphine as a catalyst, allowing for a significant increase in diluent monomer content to over 50%, resulting in a resin with fast curing speed, good toughness, and low shrinkage.
The lactic acid-based resin improves the operability and reduces costs by enhancing mechanical properties and chemical resistance, enabling clear printing of complex objects with high adhesion and flexibility, while maintaining transparency and resistance to water, acids, and alkalis.
Smart Images

Figure CN119081069A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a light-curing 3D printing UV resin based on lactic acid, a preparation method and application thereof, and belongs to the fields of green chemical industry and polymer materials. Background Art
[0002] 3D printing technology was previously known as rapid prototyping (RP) technology. It is a technology that uses the principle of additive manufacturing (MIM or AM) to achieve rapid manufacturing of parts with arbitrary complex spatial shapes. Its basic principle is layer-by-layer manufacturing, which adds materials layer by layer to generate three-dimensional entities. It integrates the latest developments in computers, lasers, precision machinery, micro-nano manufacturing, materials science, and control science and technology, and can automatically and quickly transform design ideas into physical prototypes with certain structural functions, thereby facilitating rapid evaluation, modification, and functional testing of product designs, effectively shortening the product development cycle.
[0003] Usually, UV light-curing resin has a high viscosity, and it is difficult to construct as a 3D printing material. Therefore, light-curing diluent is needed as a chemical to reduce the viscosity of UV light-curing coatings. It can increase the fluidity and coating properties of the coating, thereby improving the quality of the coating. However, the amount of light-curing diluent that can be added to 3D printing materials is very limited, only 6-8% of the mass of the UV resin, and at most 10%. If the diluent monomer continues to increase, its strength, adhesion and other properties will not meet the use requirements. Summary of the invention
[0004] The invention relates to a photocurable 3D printing UV resin based on lactic acid, a preparation method and an application thereof. The lactic acid resin photocurable material prepared by the photocurable 3D printing UV resin based on lactic acid of the invention has fast curing speed, good toughness and low shrinkage. While ensuring mechanical properties (such as strength and adhesion) and chemical resistance, the usage of diluent monomers is greatly increased to more than 50%, thereby improving the operability of the photocurable material and reducing the cost. The material can be applied to photocurable 3D printing, so that the load object can be clearly printed.
[0005] In order to solve the above technical problems, the technical solutions adopted by the present invention are as follows:
[0006] A light-curing 3D printing UV resin based on lactic acid, the molecular structure is:
[0007]
[0008] The value of n is 0-2.
[0009] The above-mentioned light-curing 3D printing UV resin based on lactic acid is prepared by reacting lactic acid, bisphenol A epoxy resin and acrylic acid, wherein the molar ratio of lactic acid: bisphenol A epoxy resin: acrylic acid is (0.3-1): 1: 1.
[0010] In order to ensure the resin performance, the bisphenol A epoxy resin is at least one of E20, E35, E40, E42, E44, E51, and E54, preferably E44, E51, and E54, and more preferably E54.
[0011] The preparation method of the light-curing 3D printing UV resin based on lactic acid, under solvent-free conditions, uses p-hydroxyanisole as an inhibitor and triphenylphosphine as a catalyst, and heats lactic acid, bisphenol A epoxy resin and acrylic acid to react in the dark to obtain the light-curing 3D printing UV resin based on lactic acid.
[0012] As one specific implementation scheme, the above preparation method comprises the following steps:
[0013] 1) mixing acrylic acid, bisphenol A epoxy resin, inhibitor p-hydroxyanisole and catalyst triphenylphosphine uniformly, reacting at 80-90° C. in the dark until the acid value AV≤1 to obtain an intermediate product;
[0014] 2) adding lactic acid to the intermediate product obtained in step 1), reacting at 80-90° C. in the dark until the acid value AV≤3, to obtain a lactic acid photocurable UV resin.
[0015] In the above preparation method, when all the carboxyl groups of acrylic acid have reacted, the reaction of step 1) is completed; when all the carboxyl groups of lactic acid have reacted, the reaction of step 2) is completed.
[0016] The above method is simple, safe and easy to control.
[0017] In the above step 1), the reaction time is 3 to 8 hours; in the step 2), the reaction time is 8 to 10 hours.
[0018] The above steps 1) and 2) are both carried out under the protection of nitrogen.
[0019] The amount of the polymerization inhibitor p-hydroxyanisole accounts for 0.1% to 0.3% of the total mass of acrylic acid, bisphenol A epoxy resin and lactic acid, and the amount of the catalyst triphenylphosphine accounts for 0.3% to 0.5% of the total mass of acrylic acid, bisphenol A epoxy resin and lactic acid.
[0020] The above-mentioned light-curing 3D printing UV resin based on lactic acid is used to prepare a lactic acid resin light-curing material, and the prepared lactic acid resin light-curing material is used for coating or 3D printing.
[0021] When used for coatings, a smooth, transparent, high-adhesion coating can be obtained. The coating has excellent flexibility, impact resistance greater than 50kg·cm, flexibility ≤1mm, and can adapt to at least 1mm bending without breaking. In terms of water resistance, even after 48 hours of immersion in water, the coating still maintains its original gloss without any signs of loss of gloss, whitening, bubbles or shedding.
[0022] The preparation method of the lactic acid resin photocurable material is as follows: uniformly mix the lactic acid-based photocurable 3D printing UV resin, the acrylate diluent monomer and the photoinitiator TPO, remove bubbles in an environment of 20 to 30° C., and irradiate with ultraviolet light to form the lactic acid resin 3D printing photocurable material.
[0023] The mass dosage of the above-mentioned acrylate diluent monomer is 15-60% of the mass of the light-curing 3D printing UV resin based on lactic acid, and the mass dosage of the photoinitiator TPO is 1%-5% of the sum of the mass of the light-curing 3D printing UV resin based on lactic acid and the acrylate diluent monomer.
[0024] The acrylic acid ester diluent monomer is at least one of 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, 4-acryloylmorpholine or isobornyl acrylate, preferably isobornyl methacrylate.
[0025] The technologies not mentioned in the present invention are all referred to the prior art.
[0026] The beneficial effects of the present invention are:
[0027] The present invention is based on the light-curing 3D printing UV resin of lactic acid, uses bisphenol A epoxy resin compounds, epoxy ring opening under the action of a catalyst, and reacts with acrylic acid epoxy ring opening to generate acrylic acid intermediate compounds, which are then reacted with lactic acid to generate modified epoxy resins, which can effectively reduce viscosity and can be applied to coatings or 3D printing. The resulting product has fast curing speed, good toughness, low shrinkage, high transparency, and excellent acid resistance, alkali resistance, and salt resistance. The synthesis method is simple, safe, easy to control, and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a physical picture of the preparation of the lactic acid light-curing 3D printing UV resin of the present invention;
[0029] Figure 2 This is the infrared spectrum of the lactic acid photocuring 3D printing UV resin of the present invention;
[0030] Figure 3 The UV images of the diluent monomer and lactic acid photocurable 3D printing UV resin of the present invention with different mass fractions are shown;
[0031] Figure 4 The mechanical properties of the mixture of different mass fractions of diluent and lactic acid light-curing 3D printing UV resin of the present invention;
[0032] Figure 5 TG graphs of different mass fractions of diluent monomer and lactic acid photocurable 3D printing UV resin of the present invention;
[0033] Figure 6 This is a physical picture of the 3D printing of the lactic acid light-curing 3D printing UV resin of the present invention. DETAILED DESCRIPTION
[0034] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0035] Example 1
[0036] Acrylic acid (7.2 g, 0.1 mol), epoxy resin E54 (37.03 g, 0.1 mol), inhibitor 4-methoxyphenol (0.0885 g), and catalyst triphenylphosphine (0.1769 g) were added into a 250 mL three-necked flask, and the mixture was heated to 70°C and stirred at a speed of 200 rad / min for 10 min to completely dissolve the inhibitor; the temperature was adjusted to 90°C for reaction under light-proof conditions, and the degree of reaction was monitored by detecting the acid value of the reaction. After 5 hours of reaction, the acid value was less than 1 and no longer changed, and an intermediate product was generated. Lactic acid (9 g, 0.1 mol) was added, and the reaction was carried out at 90°C in the dark (light-proof conditions). The degree of reaction was monitored by detecting the acid value of the reaction. After 10 hours of reaction, the acid value no longer changed and was less than 3, and lactic acid light-curing UV resin (light-curing 3D printing UV resin based on lactic acid) E54-LA-ACA was generated. Figure 1 As shown, the above reactions were all carried out under the protection of nitrogen.
[0037] Figure 2 FT-IR spectra of the raw materials ACA, epoxy resin E54, lactic acid LA and the final product. The stretching vibration of -OH is at 3446cm -1 A broad peak was observed, and the characteristic peak of the epoxy group disappeared at 910 cm-1. In addition to the hydroxyl group contained in lactic acid, the epoxy ring opening would generate hydroxyl groups, indicating that the epoxy group was completely ring-opened, 1719 cm-1 -1 The absorption peak of -C=O- indicates that the carboxylic acid has completely reacted with the epoxy group and the acid carbonyl group has completely converted into the ester carbonyl group. The stretching vibration of the -C=C- bond is generally at 1695 cm -1 From the above, we can get that the compound synthesized in this experiment contains a -C=C- bond and does not contain an epoxy group, and its structure is:
[0038]
[0039] Example 2
[0040] Preparation of light-curable materials:
[0041] Accurately weigh 3.192 g of photoinitiator TPO with an analytical balance, add 53.2 g of lactic acid photocurable UV resin prepared in Example 1, add 26.6 g of diluent isobornyl methacrylate IBOA, heat to 50° C., stir and mix thoroughly, pour into a polytetrafluoroethylene mold, remove bubbles at 20-30° C., and evenly coat on a corona-treated polypropylene film with a wire rod coater. The coating layer has a thickness of 10 μm. Place the coating under a UV lamp for 2 seconds (the UV lamp irradiation intensity is about 1036 mJ / cm 2 , distance 21cm), solidified to obtain E54-LA-ACA / IBOA50.
[0042] The prepared coating is not only smooth and transparent, but also has strong adhesion to the substrate, reaching level 0. In addition, the coating has excellent flexibility, impact resistance greater than 50kg·cm, flexibility ≤1mm, and can adapt to at least 1 mm of bending without breaking. In terms of water resistance, even after 48 hours of immersion in water, the coating still maintains its original gloss, without any signs of gloss loss, whitening, bubbles or shedding. At the same time, the same method was used to add different mass fractions of the diluent monomer isobornyl methacrylate (IBOA) for comparison. UV spectroscopy tests were performed on diluent monomers with different mass fractions, such as Figure 3 As shown in the figure, the transparency is above 85%.
[0043] After curing, the uniaxial tensile test was carried out to test its mechanical properties. Figure 4 As shown by Figure 4 It can be seen that the addition of 30% diluent monomer isobornyl methacrylate (IBOA) can well balance tensile strength and strain, showing better tensile strength. It can be seen that the application significantly increases the amount of diluent monomer, and the amount of diluent monomer can reach more than 30%, and can still better balance tensile strength (42Mpa) and elongation at break (up to 12%), while achieving 0-level adhesion, greatly improving the operability of the photocurable material. The existing diluent monomer can only reach 6-8% of the mass of UV resin, and can only reach 10% at most. If the diluent monomer continues to increase, the strength will decrease; and if the amount of diluent monomer is small, the operability of the material will deteriorate, increasing the difficulty of operation, thereby affecting the quality, and the reduction of the amount of diluent monomer means an increase in the amount of UV resin, thereby increasing the cost. Figure 3 and Figure 4In the figure, 10% means that the mass dosage of isobornyl methacrylate (IBOA) is 10% of the mass of the lactic acid photocurable UV resin, and the other similar expressions have similar meanings. TG tests were performed on diluent monomers with different mass fractions, such as Figure 5 shown.
[0044] Example 3
[0045] Testing the adhesion of light-curing materials on tinplate:
[0046] The preparation of the photocurable material refers to Example 2. As described in Example 2, the adhesion of the photocurable material on the plastic substrate can reach level 0. This example tests the adhesion of the photocurable material on tinplate. The photocurable material is attached to the tinplate. The coating layer thickness is 10 μm. The adhesion of E54-LA-ACA / IBOA50 (the mass dosage of IBOA is 50% of the mass of the lactic acid photocurable UV resin) reaches level 1. It can be seen that this photocurable material also has good adhesion on the metal substrate, so that it can better adhere to the photocurable 3D printing platform.
[0047] Example 4
[0048] The following parameters were used for printing using the CREATY SKY light-curing 3D printer from Shenzhen CREATY 3D Technology Co., Ltd.: initial exposure 40s, light-off delay 4s, printing exposure 2.2s, printing rise height 7mm, motor speed 1mm / s, bottom exposure layer 3 layers. E54-LA-ACA / IBOA50 was able to clearly print complex objects on the tinplate 3D printing platform. Figure 6 .
[0049] Example 5
[0050] To conduct the chemical resistance test, the photocurable material was first cut into small pieces of 2 cm × 2 cm and their initial weight was measured. 2 S0 4 The material was immersed in 10wt% aqueous solution, 10wt% NaOH aqueous solution, and 3wt% NaCl aqueous solution at room temperature for 48 hours. After the immersion is completed, take out the material block, wipe the surface solution with a clean cloth, and measure the weight again. By comparing the weight of the material before and after immersion, the mass retention rate of the material can be calculated. This ratio is used to evaluate the material's tolerance to acids, alkalis, and salts. The mass retention rate of the light-curing resin under these test conditions is more than 99.9%, and the resin has excellent acid resistance, alkali resistance, and salt resistance.
[0051] According to the description of the present invention, professionals in the relevant field can make appropriate adjustments and changes to the embodiments. Therefore, the protection scope of the present invention should not be limited to the aforementioned embodiments, and some improvements and changes of the present invention should also be considered to be within the protection of the claims. In addition, although certain specific terms are used in the description, these terms are only used for the convenience of description and do not impose any limitation on the scope of application of the present invention.
Claims
1. A light-curing 3D printing UV resin based on lactic acid, Features: The molecular structure is: The value of n is 0-2.
2. The light-curable 3D printing UV resin based on lactic acid as claimed in claim 1, Features: The invention is prepared by the reaction of lactic acid, bisphenol A epoxy resin and acrylic acid, wherein the molar ratio of lactic acid: bisphenol A epoxy resin: acrylic acid is (0.3-1):1:
1.
3. The light-curable 3D printing UV resin based on lactic acid as claimed in claim 2, It is characterized in that: It is characterized in that: The bisphenol A epoxy resin is at least one of E20, E35, E40, E42, E44, E51, and E54.
4. A method for preparing a light-curable 3D printing UV resin based on lactic acid according to any one of claims 1 to 3, Features: Under solvent-free conditions, with p-hydroxyanisole as inhibitor and triphenylphosphine as catalyst, lactic acid, bisphenol A epoxy resin and acrylic acid were heated and reacted in the dark to prepare the lactic acid-based light-curing 3D printing UV resin.
5. The preparation method according to claim 4, Features: The steps include: 1) mixing acrylic acid, bisphenol A epoxy resin, inhibitor p-hydroxyanisole and catalyst triphenylphosphine uniformly, reacting at 80-90° C. in the dark until the acid value AV≤1 to obtain an intermediate product; 2) adding lactic acid to the intermediate product obtained in step 1), reacting at 80-90° C. in the dark until the acid value AV≤3, to obtain a lactic acid photocurable UV resin.
6. The preparation method according to claim 5, Features: In step 1), the reaction time is 3 to 8 hours; in step 2), the reaction time is 8 to 10 hours.
7. The preparation method according to claim 5 or 6, Features: The reaction of step 1) and step 2) is carried out under the protection of nitrogen; the amount of the polymerization inhibitor p-hydroxyanisole accounts for 0.1% to 0.3% of the total mass of acrylic acid, bisphenol A epoxy resin and lactic acid, and the amount of the catalyst triphenylphosphine accounts for 0.3% to 0.5% of the total mass of acrylic acid, bisphenol A epoxy resin and lactic acid.
8. A use of the lactic acid-based light-curing 3D printing UV resin according to any one of claims 1 to 3, Features: Used to prepare lactic acid resin photocuring materials, and the prepared lactic acid resin photocuring materials are used for coatings or 3D printing.
9. The use according to claim 8, Features: The preparation method of the lactic acid resin photocurable material is as follows: uniformly mix the lactic acid-based photocurable 3D printing UV resin, the acrylate diluent monomer and the photoinitiator TPO, remove bubbles in an environment of 20 to 30° C., and irradiate with ultraviolet light to form the lactic acid resin 3D printing photocurable material.
10. The method for preparing the lactic acid resin photocurable material according to claim 8, Features: The mass dosage of the acrylate diluent monomer is 15-60% of the mass of the light-curing 3D printing UV resin based on lactic acid, and the mass dosage of the photoinitiator TPO is 1%-5% of the sum of the mass of the light-curing 3D printing UV resin based on lactic acid and the acrylate diluent monomer; the acrylate diluent monomer is at least one of 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, 4-acryloylmorpholine or isobornyl acrylate.
Citation Information
Patent Citations
Photocurable resin and photocurable resin composition
CN102388077A
Water-based acrylic acid-epoxy-polyurethane dispersoid and alcohol-rubbing-resistant and alkali-resistant coating
CN111154042A
Polylactic acid-based macromonomer as well as preparation method and application thereof
CN112898497A
UV photocuring 3D printing resin as well as preparation method and application thereof
CN115819687A
Process for preparing high molecular weight poly(lactic acid) by melt polycondensation