Indigo dye-based porous organic polymer, synthesis and application of indigo dye-based porous organic polymer in lithium ion battery positive electrode material
Through Sonogashira coupling reaction and multi-wall carbon nanotube composite, an indigo porous organic polymer electrode material was developed, which solved the problem of high resource consumption and cost of the positive electrode material synthesis of lithium-ion batteries, and achieved high performance and low cost electrode materials , fills the gap in indigo-based porous polymers in lithium-ion battery applications.
Patent Information
- Application Number
- CN202410615994.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-17
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-05-17
AI Technical Summary
The existing lithium-ion battery cathode materials consume mineral resources, generate carbon emissions and are costly during the synthesis process. Indigo dye-based porous organic polymers have not been developed in battery applications, and lack high open circuit voltage and dual electron redox reactions. Mechanism material.
The indigo porous organic polymer was synthesized through the Sonogashira coupling reaction and combined with multi-wall carbon nanotubes to prepare a new electrode material with high specific surface area and good conductivity, using indigo molecules with 1,3,5-triacetylene benzene monomers. The body is copolymerized and combined with conductive carbon materials to form a composite material.
The new indigo organic electrode material that achieves high rate performance and excellent cycle performance is simple to synthesis, rich resources and low price, filling the gap in indigo-based porous polymers in lithium-ion battery applications.
Smart Images

Figure CN119081072A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion battery positive electrode materials, and relates to the synthesis of an indigo dye molecule-based porous organic polymer and its application in lithium ion battery positive electrode materials. Background Art
[0002] The growing demand for energy storage has driven the rapid development of lithium-ion batteries and has dominated the electronic product market. Electrodes, as the core components of battery equipment, not only determine the battery capacity, but are also an important factor affecting whether the battery can achieve long life, low cost and reliable safety. Currently, the electrode materials used in batteries are mainly divided into inorganic electrode materials and organic electrode materials. Inorganic electrode materials (such as LiCoO 2 、LiMn 2 O 4 、LiFePO 4 ) is synthesized at the expense of consuming mineral resources and generating carbon emissions, and its production consumes a lot of energy. Organic electrode materials usually store lithium based on the charge conversion of active functional groups. They are rich in sources, diverse in structure, easily regulated in function, and have high theoretical specific capacity. They can simultaneously achieve high energy density, high cycle stability, and high power density of batteries. In this case, organic materials are a better choice as electrode materials.
[0003] Among organic materials, porous organic polymers (POPs) have large specific surface areas and pores. When used as electrodes, they can provide more active centers for the storage and diffusion of ions, thereby improving the storage performance of batteries. They have great potential in developing batteries with excellent electrochemical performance. In particular, dye-based POPs, because dyes contain carbonyl groups connected by functional conjugated bonds, are abundant in resources and environmentally friendly, and dye-based porous polymers containing carbonyl structures combine the advantages of porous organic materials and reduced dyes, and have received extensive attention in the fields of material chemistry and organic electronics.
[0004] Indigo, pyrenetetraketone, pyrrolopyrroledione, naphthalene diimide, perylene diimide and anthraquinone dyes are common dyes containing active carbonyl functional groups. In recent years, these dye-based porous organic polymers with different structures have been developed and applied to battery electrode materials. However, indigo dye-based porous organic polymers have not yet appeared at this stage. Indigo dyes have high open circuit voltage, high carrier mobility and two-electron redox reaction mechanism. Due to the introduction of nitrogen atoms, the indigo structure is more electron-deficient, the lowest unoccupied molecular orbital energy level is lower, and the planarity is better, which has great advantages as an electron transport material. Based on this vacancy, we have developed indigo dye-based porous organic polymer materials and used them as new lithium-ion battery electrode materials. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing an indigo dye-based porous organic polymer, study its application in the positive electrode of a lithium ion battery, and fill the gap in the application of indigo-based porous polymers in lithium ion batteries.
[0006] The technical solution of the present invention:
[0007] An indigo dye-based porous organic polymer having the following structural formula:
[0008]
[0009] A method for preparing an indigo-based porous organic polymer, comprising the following steps:
[0010] Step 1, using 4-bromo-2-nitrobenzaldehyde, acetone, water and alkaline solution as raw materials to react and synthesize 6,6'-dibromoindigo;
[0011] Step 2, using 6,6'-dibromoindigo, 4-dimethylaminopyridine, di-tert-butyl carbonate and N,N-dimethylformamide as raw materials to react and synthesize 6,6'-dibromo-1,10-dicarboxylic acid di-tert-butyl indigo;
[0012] Step 3, using 6,6'-dibromo-1,10-dicarboxylic acid di-tert-butyl indigo as a building monomer, and carrying out a Sonogashira coupling reaction with 1,3,5-triethynylbenzene in a mixed solvent in the presence of a catalyst, and purifying the reaction product after the reaction to prepare a porous organic polymer based on indigo molecules.
[0013] In step 1, the mass ratio of 4-bromo-2-nitrobenzaldehyde to water is 1:50, the volume ratio of acetone to water is 1:1-1:1.2, the alkaline solution is a 2M NaOH solution, the amount of dropwise addition is to adjust the pH value to 9-10, and the reaction conditions are 16-25° C. for 10-15 hours;
[0014] In step 2, the molar ratio of 4-dimethylaminopyridine to 6,6'-dibromoindigo is 1:1.7-1:2, the molar ratio of 6,6'-dibromoindigo to di-tert-butyl carbonate is 1:2-1:5.3, and the mass ratio of 6,6'-dibromoindigo to N,N-dimethylformamide is 1:5.6-1:5.7; the temperature when adding di-tert-butyl carbonate is 0°C, and it needs to be added in two times, and the reaction conditions are 16-25°C for 20-24h;
[0015] The catalyst in step 3 is a mixture of tetrakis(triphenylphosphine)palladium and cuprous iodide, the molar ratio of the two catalysts is 1:40, and the mixed solvent is a mixture of N,N-dimethylformamide and triethylamine, and the volume ratio is 1:1; the molar ratio of 6,6'-dibromo-1,10-dicarboxylic acid di-tert-butyl indigo to 1,3,5-triethynylbenzene is 1.5:1, the molar ratio of cuprous iodide to 6,6'-dibromo-1,10-dicarboxylic acid di-tert-butyl indigo is 1:10, and the mass ratio of 6,6'-dibromo-1,10-dicarboxylic acid di-tert-butyl indigo to N,N-dimethylformamide is 1:15-1:16;
[0016] In step 3, the reaction conditions are degassing under freezing pump thawing, purging with argon, heating to 80-110°C three times, and reacting for 48-96 hours. The purification treatment is washing with methanol, water, chloroform and acetone in sequence, Soxhlet extraction with anhydrous methanol and drying.
[0017] A composite material of an indigo-based porous organic polymer and a conductive carbon material is applied to a positive electrode material of a lithium-ion battery, wherein the conductive carbon material is a multi-walled carbon nanotube.
[0018] In the composite material, the mass percentage of the multi-walled carbon nanotubes is 20% to 40%.
[0019] Beneficial effects of the present invention: The present invention uses the Sonogashira coupling reaction to copolymerize indigo molecules containing carbonyl structures with 1,3,5-triethynylbenzene monomers to synthesize a new type of porous organic polymer containing indigo dye in the molecular chain. The material has a large specific surface area, which is also the first porous organic polymer based on the indigo structure. Then, the porous organic polymer is in situ polymerized using multi-walled carbon nanotubes to obtain a composite material with good conductivity, and a new type of indigo organic electrode material with high rate performance and good cycle performance is developed. Compared with traditional inorganic materials, its synthesis is simple, does not require high temperature, and the dye material is abundant in source, low in price, and can be applied industrially. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 For the material in Example 2 1 H NMR spectrum;
[0021] Figure 2 is the infrared spectra of the materials in Example 3 and Example 4;
[0022] Figure 3 are scanning electron microscope (SEM) images of the materials in Example 3 and Example 4, wherein (a) is the SEM image of the material in Example 3, and (b) is the SEM image of the material in Example 4;
[0023] Figure 4The XRD spectra in Examples 3 and 4 are shown below:
[0024] Figure 5 The nitrogen adsorption spectra of the materials in Examples 3 and 4 are shown in Figures 1 and 2, wherein (a) is an isothermal adsorption-desorption curve of the materials in Examples 3 and 4, and (b) is a pore size distribution diagram of the materials in Examples 3 and 4;
[0025] Figure 6 The material in Example 4 is 0.1 mV s -1 Cyclic voltammetry test diagram under scanning rate;
[0026] Figure 7 This is a rate performance test diagram of the material in Example 4;
[0027] Figure 8 This is the cycle performance diagram of the material in Example 4 at 0.5C. DETAILED DESCRIPTION
[0028] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and technical solutions.
[0029] Example 1
[0030] 4-Bromo-2-nitrobenzaldehyde (2 g, 8.7 mmol) was dissolved in acetone (90 mL), and then water (100 mL) was slowly added. The mixture was stirred at room temperature overnight and filtered. The solid was washed with excess acetone and deionized water, and then vacuum dried to obtain 1.32 g of purple powder 6,6'-dibromoindigo (INO) with a yield of 72.1%. The reaction formula is as follows:
[0031]
[0032] Due to the poor solubility of INO, in order to increase the degree of polymerization, we used di-tert-butyl diformate group substitution protection to solubilize it to facilitate the polymerization reaction, and then removed the protecting group and reduced it in the subsequent heating polymerization.
[0033] Example 2
[0034] To a suspension of compound INO (0.842 g, 2.0 mmol) and 4-dimethylaminopyridine (0.147 g, 1.2 mmol) in N,N-dimethylformamide (DMF, 5 mL), di-tert-butyl carbonate (2.31 g, 10.6 mmol) was added twice at 0°C. The mixture was then stirred at room temperature for 20 hours, during which time the color of the suspension changed from dark red to bright red. The product was separated by filtration, and the residue was washed with DMF and deionized water and dried. 1.03 g of pink powder 6,6'-dibromo-1,10-dicarboxylic acid di-tert-butyl ester indigo (INO-BOC) was recrystallized from a mixture of chloroform / isopropanol with a yield of 82.7%. The reaction formula is as follows:
[0035]
[0036] The product prepared in this example 1 H NMR spectrum Figure 2 The characterization data are as follows: 1 H NMR (400 MHz, CDCl 3 ): δ=8.26(s,2H),7.61(d,J=8.1Hz,2H),7.37(dd,J=8.1,1.6Hz,2H),1.61(s,18H).
[0037] Example 3
[0038] INO-BOC (310 mg, 0.5 mmol), TEB (38 mg, 0.25 mmol), tetrakis(triphenylphosphine)palladium(0) (15 mg) and cuprous iodide (10 mg) were dissolved in DMF (5.0 mL) and Et 3 N (5.0mL). Degassing under freeze pump thawing, purging with argon, and reacting at 100°C for 48h. Then the mixture was cooled to room temperature, the precipitated polymer was filtered, and the filter cake was washed with methanol, water, chloroform and acetone respectively. Further Soxhlet extraction with methanol was performed for 48h, and the product was vacuum dried at 70°C for 24h to obtain yellow-green powder IN-TEB. Its reaction formula is as follows:
[0039]
[0040] The infrared spectrum of the product prepared in this example is as follows Figure 2 As shown, the -CH 3 , C=O and COC bond absorption peaks (3005-2925 cm -1 1767~1729cm -1 and 1295~1214cm -1) disappeared, indicating the successful synthesis of polymer IN-TEB. Figure 3 As shown in a, the polymer IN-TEB has an irregular block morphology. Figure 4 As shown in the figure, it can be seen that IN-TEB has an amorphous structure. The nitrogen adsorption and pore size distribution diagram is shown in Figure 5 As shown in the figure, it can be seen that the specific surface area of IN-TEB is 576.536m 2 g -1 The pore size is 0.524 nm. These results indicate that IB-TEB is a porous organic polymer.
[0041] Example 4
[0042] Synthesis of IB@CNT composited with multi-walled carbon nanotubes (i.e., indigo-based porous organic polymer composites): INO-BOC (310 mg), TEB (38 mg), multi-walled carbon nanotubes (69 mg), tetrakis(triphenylphosphine)palladium(0) (15 mg), and cuprous iodide (10 mg) were dissolved in DMF (5.0 mL) and Et 3 N (5.0 mL). Degassing under freeze pump thawing, purging with argon, and reacting at 100 ° C for 48 hours. Then the mixture was cooled to room temperature, the precipitated polymer was filtered, and the filter cake was washed with methanol, water, chloroform and acetone respectively. Soxhlet extraction with methanol was further performed for 48 hours, and the product was vacuum dried at 70 ° C for 24 hours to obtain black powder IB@CNT229mg, in which the mass percentage of multi-walled carbon nanotubes (doping rate) was 30wt%. Infrared ( Figure 2 ) and XRD( Figure 4 ) test verified the successful synthesis of the material. SEM analysis was performed to obtain the morphology of the powder as shown in Figure 3 As shown in b, IB@CNT is a fiber mesh with a porous structure. The nitrogen adsorption and pore size distribution are shown in Figure 5 As shown in the figure, it can be seen that the specific surface area of IN-TEB is 490.310m 2 g -1 , the pore size is 0.476nm.
[0043] The 2032 lithium-ion battery was prepared using the following process. The prepared IB@CNT polymer was used as the active material, Super P as the conductive additive, and PVDF as the binder. They were stirred in a mortar in a mass ratio of 7:2:1 in N-methyl-2-pyrrolidone (NMP) solvent to form a uniform slurry. The slurry was coated on aluminum foil using a coater and placed in a vacuum drying oven to dry overnight. Finally, a cutting machine was used to cut the electrode sheet into a circular electrode sheet with a diameter of 12 mm for use as a working electrode. A metal lithium sheet was used as the counter electrode, a 16 mm diameter Ceglard 2400 membrane was used as the battery separator, and 1M lithium hexafluorophosphate (LiPF 6 ) was dissolved in a mixed solution (1:1:1 Vol%) of dimethyl carbonate (DMC), ethylene carbonate (EC) and ethyl methyl carbonate (EMC) as the electrolyte, all in a glove box (O 2 ≤0.1ppm, H 2 O≤0.1ppm), and sealed on a sealing machine, and finally left to stand for use.
[0044] The assembled battery was tested for constant current charge and discharge curve and rate performance in the Xinwei battery test system, with a voltage range of 1.5-4V (vs Li + / Li). The cyclic voltammetry curves (CV, scan rate was 0.1 mV s -1 )Measurement.
[0045] The prepared battery was subjected to electrochemical testing, and the test results were as follows: Figure 6 As shown in the figure, the cyclic voltammetry curve of the polymer IB@CNT battery has two pairs of redox peaks, indicating that the polymer has a two-electron redox mechanism. In the electrochemical performance test, the IB@CNT battery showed a high rate performance ( Figure 7 ) and excellent cycle performance ( Figure 8 ).
[0046] The above results indicate that the novel porous organic polymer described in the present invention can be used as a very potential positive electrode material in lithium-ion batteries.
Claims
1. An indigo dye-based porous organic polymer, characterized in that: The indigo dye-based porous organic polymer has the following structural formula:
2. A method for preparing an indigo dye-based porous organic polymer, characterized in that: Here are the steps: Step 1, using 4-bromo-2-nitrobenzaldehyde, acetone, water and alkaline solution as raw materials to react and synthesize 6,6'-dibromoindigo; Step 2, using 6,6'-dibromoindigo, 4-dimethylaminopyridine, di-tert-butyl carbonate and N,N-dimethylformamide as raw materials to react and synthesize 6,6'-dibromo-1,10-dicarboxylic acid di-tert-butyl indigo; Step 3, using 6,6'-dibromo-1,10-dicarboxylic acid di-tert-butyl indigo as a building monomer, and carrying out a Sonogashira coupling reaction with 1,3,5-triethynylbenzene in a mixed solvent in the presence of a catalyst, and purifying the reaction product after the reaction to prepare an indigo dye-based porous organic polymer.
3. The preparation method according to claim 2, characterized in that: In step 1, the mass ratio of 4-bromo-2-nitrobenzaldehyde to water is 1:50, the volume ratio of acetone to water is 1:1-1:1.2, the alkaline solution is a 2M NaOH solution, and the amount of addition is to adjust the pH value to 9-10.
4. The preparation method according to claim 2, characterized in that: In step 1, the reaction conditions are 16-25° C. for 10-15 h.
5. The preparation method according to claim 2, characterized in that: In step 2, the molar ratio of 4-dimethylaminopyridine to 6,6'-dibromoindigo is 1:1.7-1:2, the molar ratio of 6,6'-dibromoindigo to di-tert-butyl carbonate is 1:2-1:5.3, and the mass ratio of 6,6'-dibromoindigo to N,N-dimethylformamide is 1:5.6-1:5.
7.
6. The preparation method according to claim 2, characterized in that: In step 2, the temperature when adding di-tert-butyl carbonate is 0°C, and it needs to be added in two times. The reaction conditions are 16-25°C and the reaction time is 20-24h.
7. The preparation method according to claim 2, characterized in that: In step three, the catalyst is a mixture of tetrakis(triphenylphosphine)palladium and cuprous iodide, the molar ratio of tetrakis(triphenylphosphine)palladium to cuprous iodide is 1:40, the mixed solvent is a mixture of N,N-dimethylformamide and triethylamine, and the volume ratio is 1:1; the molar ratio of 6,6'-dibromo-1,10-dicarboxylic acid di-tert-butyl indigo to 1,3,5-triethynylbenzene is 1.5:1, the molar ratio of cuprous iodide to 6,6'-dibromo-1,10-dicarboxylic acid di-tert-butyl indigo is 1:10, and the mass ratio of 6,6'-dibromo-1,10-dicarboxylic acid di-tert-butyl indigo to N,N-dimethylformamide is 1:15-1:
16.
8. The preparation method according to claim 2, characterized in that: In step three, the reaction conditions are degassing under thawing with a freeze pump, purging with argon, heating to 80-110°C three times, and reacting for 48-96 hours; the purification treatment is washing with methanol, water, chloroform and acetone in sequence, Soxhlet extraction with anhydrous methanol and drying.
9. Application of a composite material of indigo dye-based porous organic polymer and conductive carbon material in positive electrode materials of lithium-ion batteries.
10. The use according to claim 9, characterized in that: The conductive carbon material is multi-walled carbon nanotubes, and the mass percentage of the multi-walled carbon nanotubes in the composite material is 20% to 40%.
Citation Information
Patent Citations
Conjugated microporous polymer and application thereof as solid electrolyte in lithium ion battery
CN115449055A
Application of indigo compound as battery negative electrode material and aqueous battery based on indigo compound
CN117712374A
Water-in-oil cosmetic composition with maximized moisture
KR102269866B1