Resin microsphere modified polylactic acid oligomer and polylactic acid composite material
By blending the polylactic acid oligomer modified by resin microspheres with commercial polylactic acid, the problem of the decrease in strength of polylactic acid materials when improving toughness is solved, synchronous enhancement and toughening of polylactic acid materials are achieved, and the overall material is improved. performance.
Patent Information
- Application Number
- CN202411348845.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-26
AI Technical Summary
The problem of the strength of existing polylactic acid materials decreasing when improving toughness, especially when adding dehydrated lactic acid units, the toughness is increased but the strength is reduced.
The polylactic acid oligomer modified with resin microspheres is formed by reacting lactide monomer with alcohol hydroxy initiator to form a branched structure, combining resin microspheres with different structures, adjusting the polymerization degree and structure to achieve polylactic acid oligomerization. The diversified adjustment of the substances forms a controlled polymer with a specific structure and blends it with commercial polylactic acid to form a composite material.
The toughness and strength of polylactic acid materials are improved, and the toughening is synchronously enhanced without adding additional components, destroying the linear polylactic acid chain entanglement structure, promoting molecular chain movement, improving crystallization performance, and enhancing the overall performance of the material.
Smart Images

Figure CN119081079A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a polylactic acid oligomer modified by resin microspheres and a polylactic acid composite material. Background Art
[0002] Biomass-based polylactic acid (PLA) is a thermoplastic polyester made from renewable resources. Due to its excellent biodegradability and non-toxicity, it has been widely used in the field of disposable tableware and packaging materials. In addition, due to its excellent mechanical strength, PLA is also widely used to develop durable structural products in engineering applications. However, the brittleness and low impact strength of PLA severely limit its widespread application as a durable material.
[0003] At present, chemical modification and physical blending are the main methods to improve the toughness of PLA. In terms of chemical modification, flexible molecular chains are incorporated into PLA through copolymerization or grafting reaction to achieve toughening of PLA. However, its modification process is usually complicated, expensive and time-consuming. In contrast, physical blending is a more direct and easier method to increase the toughness of PLA by introducing plasticizers, rigid fillers, flexible polymers or rubbers, and multi-branched homogeneous polymers. However, the physical blending method also has certain limitations. For example, plasticizers will migrate to the surface of PLA products during long-term use, causing embrittlement of the products. Although the addition of rigid fillers, flexible polymers or rubbers cannot migrate, they have poor compatibility with the PLA matrix, resulting in a decrease in the mechanical strength and modulus of PLA products. Homogeneous branched polymers composed of dehydrated lactic acid units have good compatibility with the PLA matrix, and their large free volume is conducive to the migration of PLA chains to complete toughening, but these methods inevitably sacrifice the mechanical strength of PLA products to a certain extent. Therefore, the simultaneous strengthening and toughening of PLA remains a challenge. Summary of the invention
[0004] The purpose of the present invention is to provide a polylactic acid oligomer modified with resin microspheres and a polylactic acid composite material, which solves the problem that when the existing polymer containing dehydrated lactic acid units is used for PLA modification, the toughness is improved but the strength is reduced as the addition amount increases.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A polylactic acid oligomer modified by resin microspheres, and its preparation method is as follows:
[0007] a) taking lactide monomer, resin microsphere initiator and catalyst and melting them at 100-120° C. to obtain a mixture, wherein the molar ratio of alcohol hydroxyl group in the resin microsphere initiator to lactide monomer is 1-15:100;
[0008] b) reacting the mixture obtained in step a) at 115-130° C. under an inert gas atmosphere and stirring to obtain a crude product;
[0009] c) cooling, purifying and drying the crude product obtained in step b) to obtain a polylactic acid oligomer modified with resin microspheres;
[0010] The resin microspheres are phenolic resin microspheres containing a plurality of alcohol hydroxyl initiating groups.
[0011] The preparation method of the polylactic acid oligomer modified by resin microspheres uses lactide monomer as the starting material. Under the action of initiator and catalyst, the monomer triggers the ring-opening polymerization mechanism to generate the branched structure of the dehydrated lactic acid repeating unit. The alcoholic hydroxyl groups at different positions in the resin microsphere initiator provide the branch growth center, thereby realizing the synthesis of the polylactic acid oligomer modified by resin microspheres. In the process, the degree of polymerization of the dehydrated lactic acid repeating unit is adjusted by adjusting the molar ratio of the alcoholic hydroxyl group to the lactide monomer in the resin microsphere initiator; the structure of the polylactic acid oligomer modified by the resin microspheres is adjusted by selecting resin microspheres with different structures, so as to realize diversified adjustment. The degree of polymerization in the branched chain of the polylactic acid oligomer modified by the resin microspheres is 63-91, and the corresponding single-arm number average molecular weight of the polylactic acid oligomer modified by the resin microspheres is 1000-10000 g / mol. Preferably, the degree of polymerization is 55-90, and the single-arm number average molecular weight is 4000-6500 g / mol. The ring-opening polymerization reaction of the invention belongs to the coordination-insertion polymerization mechanism, the reaction system is mild and efficient, side reactions are few, the relative molecular mass distribution of the obtained resin microsphere-modified polylactic acid oligomer is narrow, and the controllable polymerization of polylactic acid with a specific structure can be realized.
[0012] Specifically, step b) is reacted at 115-130° C. for 12-48 hours.
[0013] Specifically, in step c), the crude product obtained in step b) is cooled, dissolved in dichloromethane, purified by precipitation with icy methanol, and dried under vacuum at 40-50° C. for 24-48 hours.
[0014] The resin microspheres are phenolic resin microspheres containing multiple alcohol hydroxyl initiating groups synthesized by a hydrothermal method of a phenolic compound and formaldehyde (or hexamethylenetetramine) at 80-170°C, and are prepared by a disclosed method. The phenolic compound is an organic substance containing phenolic hydroxyl groups, including but not limited to one or more of phenol, catechol, resorcinol, xylenol, catechin and gallic acid. The phenolic resin microspheres include but are not limited to one or more of xylenol-formaldehyde resin microspheres, catechin-formaldehyde resin microspheres, gallic acid-formaldehyde resin microspheres, phenol-formaldehyde resin microspheres, catechol-formaldehyde resin microspheres, and resorcinol-formaldehyde resin microspheres.
[0015] The specific preparation method of formaldehyde-phenol resin microspheres is to prepare PFM by a simple one-step hydrothermal method. Phenol and hexamethylenetetramine are dissolved in deionized water (400mL) containing surfactant polyethylene glycol (0.02g) at a molar ratio of 2:1, and magnetically stirred at room temperature for 20min. The prepared solution is poured into a hydrothermal reactor and sealed, and reacted at 160°C for 6h. After cooling to room temperature, the reaction product is collected to obtain phenolic resin microspheres. Among them, hexamethylenetetramine is decomposed into formaldehyde and ammonia by heat, which is beneficial to the phenolic reaction.
[0016] The lactide monomer is any one of L-lactide, D-lactide and meso-lactide.
[0017] The catalyst is any one of 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD), stannous octoate, stannous chloride, cycloalkoxytin, lithium chloride, and aluminum isopropoxide. The molar ratio of the catalyst to the lactide monomer is 1-5:1000. The catalyst used in the present invention has high catalytic activity, mild reaction conditions, short reaction time, high conversion rate, small catalyst dosage, no organic solvent is used in the synthesis process, no yield and cost loss caused by solvent volatilization, good economic benefits, high controllability in operation, convenient production and regulation, good applicability to different conventional commercial polylactic acids, and can effectively promote the development and application of polylactic acid in the field of engineering materials.
[0018] A polylactic acid composite material is prepared by blending 1-15% by mass of a polylactic acid oligomer modified with resin microspheres and 85-99% of commercial polylactic acid.
[0019] It should be noted that the resin microsphere-modified polylactic acid oligomer and commercial polylactic acid are vacuum dried at 70-90° C. for 12-24 hours before blending to remove moisture and avoid the influence of moisture on subsequent processing.
[0020] It should be noted that the blending process includes but is not limited to one or more of casting, injection molding, foaming, and phase separation.
[0021] Preferably, the number average molecular weight of the commercial polylactic acid is 8-15×10 4 g / mol, and a melt index of 30-85 g / 10 min. The commercial polylactic acid of the present invention adopts conventional linear polylactic acid, which is cheap, has many sources, is easy to obtain, and is convenient for application.
[0022] The beneficial effects of the present invention are as follows: resin microspheres with abundant alcohol hydroxyl initiation sites are used as initiators to react with lactide monomers to synthesize polylactic acid oligomers modified by resin microspheres; during blending and modification, the branched structure of the polylactic acid oligomers modified by resin microspheres can destroy the chain entanglement structure of linear polylactic acid; its unique topological structure can generate a larger free volume to promote the movement of linear polylactic acid molecular chains, achieve plasticization, and thus improve the toughness of commercial polylactic acid; on the other hand, due to its excellent heterogeneous nucleation ability, it can promote the crystallization of commercial polylactic acid to achieve enhancement, and achieves the simultaneous enhancement and toughening of commercial polylactic acid without adding additional components such as compatibilizers. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the reaction equation for preparing the resin microsphere-modified polylactic acid oligomer in Example 1.
[0024] Figure 2 This is the reaction equation for preparing the resin microsphere-modified polylactic acid oligomer in Example 2.
[0025] Figure 3 This is the reaction equation for preparing the resin microsphere-modified polylactic acid oligomer in Example 3.
[0026] Figure 4 Elongation at break and yield strength of the reinforced and toughened polylactic acid composite material prepared in Example 1.
[0027] Figure 5 The toughness work and Young's modulus of the reinforced and toughened polylactic acid composite material prepared in Example 1.
[0028] Figure 6 The notched impact strength and unnotched impact strength of the reinforced and toughened polylactic acid composite material prepared in Example 1.
[0029] Figure 7 This is a physical picture of the polylactic acid oligomer initiated by catechol-formaldehyde resin microspheres prepared in Example 2.
[0030] Figure 8 This is the H-NMR spectrum of the resin microsphere-modified polylactic acid oligomer PFM-OLLA prepared in Example 1.
[0031] Fig. 9 The polymerization degree of PFM-OLLA prepared at different molar ratios of alcohol hydroxyl group and lactide monomer in Example 1.
[0032] Fig.10 This is a physical picture of the polylactic acid oligomer modified with xylenol-formaldehyde resin microspheres prepared in Example 4. DETAILED DESCRIPTION
[0033] The technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1
[0035] The present embodiment relates to a method for preparing a reinforced and toughened polylactic acid, comprising the following steps:
[0036] S1 Preparation of polylactic acid oligomer modified with resin microspheres
[0037] a) taking a monomer, namely L-lactide, an initiator, namely phenol-formaldehyde resin microspheres, and a catalyst, namely stannous octoate, and melting and mixing them at 120° C. to obtain a mixed system, wherein the molar ratio of the alcohol hydroxyl group in the initiator to the lactide monomer is 2.5:100, and the molar ratio of stannous octoate to the lactide monomer is about 1:1000;
[0038] The specific preparation method of formaldehyde-phenol resin microspheres is to prepare PFM by a simple one-step hydrothermal method. Phenol and hexamethylenetetramine are dissolved in deionized water (400mL) containing surfactant polyethylene glycol (0.02g) at a molar ratio of 2:1, and magnetically stirred at room temperature for 20min. The prepared solution is poured into a hydrothermal reactor and sealed, and reacted at 160°C for 6h. After cooling to room temperature, the reaction product is collected to obtain phenolic resin microspheres. Among them, hexamethylenetetramine is decomposed into formaldehyde and ammonia by heat, which is beneficial to the phenolic reaction.
[0039] b) subjecting the mixed system obtained in step a) to a vacuum-nitrogen filling treatment for 3 cycles, and then reacting in an oil bath at 120° C. for 36 hours under a nitrogen atmosphere and magnetic stirring to obtain a crude product;
[0040] c) Cooling the crude product obtained in step b), dissolving it in dichloromethane, purifying it by precipitation with ice methanol, and vacuum drying it at 40° C. for 24 h to obtain a polylactic acid oligomer PFM modified with resin microspheres. 2.5 -OLLA;
[0041] S2: the polylactic acid oligomer PFM modified with resin microspheres obtained in step S1 2.5 -OLLA mass percentages are 0%, 2%, 4%, 6% and 8% respectively, and the rest is commercial polylactic acid weighed raw materials;
[0042] S3 takes the resin microsphere modified polylactic acid oligomer and commercial polylactic acid weighed in S2, vacuum-dries them at 80°C for 18h, mixes and stirs them evenly, and adds them into a preheated torque rheometer for melt mixing, the mixing temperature is 180°C, the mixing speed is 40r / min, the mixing time is 10min, and the mixture is cooled and pelletized to obtain modified polylactic acid masterbatch;
[0043] S4: Processing the polylactic acid masterbatch obtained in step S3 in an injection molding machine with a melting temperature of 190° C. to obtain a polylactic acid composite material.
[0044] During the experiment, under the same other conditions, the molar ratio of the alcohol hydroxyl group to the lactide monomer in the initiator was adjusted to 1:100, 2.5:100, 5:100 and 15:100, respectively, and resin microsphere-modified polylactic acid oligomers with good performance were obtained.
[0045] Figure 4-5 The elongation at break, yield strength, toughness work and Young's modulus of the reinforced and toughened polylactic acid obtained at different contents of the polylactic acid oligomer modified with resin microspheres prepared in Example 1. It can be seen that the yield strength of pure PLA is 27.9MPa, and the addition of PFM 2.5 -After OLLA, PFM 2.5 -The yield strength of OLLA / PLA composites has been effectively improved. Due to the inherent brittleness of pure PLA, its elongation at break is only 15.2%, while PFM 2.5 -The elongation at break of OLLA / PLA composites is above 60.0%. 2.5 -The addition of OLLA enhances the toughness of PLA and improves its strength. 2.5 -The Young's modulus of OLLA / PLA composites is higher than that of pure PLA (~688.0MPa). 2.5 -OLLA’s strengthening and toughening mechanism in the composites may be due to its rigid PFM component increasing the overall stiffness of the composites, its heterogeneous nucleation ability increasing the nucleation density and reducing the spherulite size, and its multi-arm structure with a large free volume enhancing the chain mobility and promoting the growth of spherulites, thus improving the crystallization properties of the composites, thereby achieving both strengthening and toughening.
[0046] Figure 6 The notched impact strength and unnotched impact strength of the reinforced and toughened polylactic acid obtained at different contents of the polylactic acid oligomer modified with resin microspheres prepared in Example 1. It can be seen that the unnotched and notched impact strengths of pure PLA are only 10.4 and 3.0 kJ / m respectively. 2 .PFM 2.5The addition of -OLLA significantly improves the unnotched and notched impact strength of the composites. This result confirms that PFM 2.5 -OLLA toughening effect on PLA matrix.
[0047] Figure 7 This is the H NMR spectrum of the polylactic acid oligomer PFM-OLLA modified with resin microspheres prepared in Example 1. Utilizing the polyhydroxy characteristics of the resin microspheres PFM, the synthesized PFM-OLLA presents a multi-arm structure. The average degree of polymerization (DP) of L-lactide L-LA on each arm is obtained at 5.20 ppm (Ia) and 4.3 ppm (Ia') according to the integrated area of the methyl proton peak (I), and the single-arm number average molecular weight is further obtained based on the degree of polymerization.
[0048] Example 2
[0049] The present embodiment relates to a method for preparing a reinforced and toughened polylactic acid, comprising the following steps:
[0050] S1 Preparation of polylactic acid oligomer modified with resin microspheres
[0051] a) taking a monomer, namely L-lactide, an initiator, namely catechol-formaldehyde resin microspheres, and a catalyst, namely stannous chloride, and melting and mixing them at 120° C. to obtain a mixed system, wherein the molar ratio of the alcohol hydroxyl group in the initiator to the lactide monomer is 1:100, and the molar ratio of stannous octoate to the lactide monomer is about 1:1000;
[0052] b) subjecting the mixed system obtained in step a) to a vacuum-nitrogen filling treatment for 3 cycles, and then reacting in an oil bath at 120° C. for 36 hours under a nitrogen atmosphere and magnetic stirring to obtain a crude product;
[0053] c) cooling the crude product obtained in step b), dissolving it in dichloromethane, purifying it by precipitation with ice methanol, and vacuum drying it at 40° C. for 24 hours to obtain a polylactic acid oligomer modified with resin microspheres;
[0054] S2 weighs the raw materials according to the following weight percentages: 4% of the polylactic acid oligomer modified with the resin microspheres obtained in step S1 and 96% of commercial polylactic acid;
[0055] S3 takes the resin microsphere-modified polylactic acid oligomer and commercial polylactic acid weighed in S2, and vacuum dries them at 80°C for 18 hours respectively, mixes them, stirs them evenly, dissolves them in dichloromethane, and after mixing them evenly, casts them into a glass mold, and evaporates them in vacuum at 40°C for 24 hours to obtain a polylactic acid composite material.
[0056] Example 3
[0057] The present embodiment relates to a method for preparing a reinforced and toughened polylactic acid, comprising the following steps:
[0058] S1 Preparation of polylactic acid oligomer modified with resin microspheres
[0059] a) taking a monomer, namely meso-lactide, an initiator, namely resorcinol-formaldehyde resin microspheres, and a catalyst, namely cycloalkoxy tin, and melting and mixing them at 120° C. to obtain a mixed system, wherein the molar ratio of the alcohol hydroxyl group in the initiator to the lactide monomer is 1:100, and the molar ratio of stannous octoate to the lactide monomer is about 1:1000;
[0060] b) subjecting the mixed system obtained in step a) to a vacuum-nitrogen filling treatment for 3 cycles, and then reacting in an oil bath at 120° C. for 36 hours under a nitrogen atmosphere and magnetic stirring to obtain a crude product;
[0061] c) cooling the crude product obtained in step b), dissolving it in dichloromethane, purifying it by precipitation with ice methanol, and vacuum drying it at 40° C. for 24 hours to obtain a polylactic acid oligomer modified with resin microspheres;
[0062] S2 weighs the raw materials according to the following weight percentages: 15% of the polylactic acid oligomer modified with the resin microspheres obtained in step S1 and 85% of commercial polylactic acid;
[0063] S3 takes the resin microsphere-modified polylactic acid oligomer and commercial polylactic acid weighed in S2, and vacuum dries them at 80°C for 18 hours respectively, mixes them, stirs them evenly, dissolves them in dichloromethane, and after mixing them evenly, casts them into a glass mold, and evaporates them in vacuum at 40°C for 24 hours to obtain a polylactic acid composite material.
[0064] Example 4
[0065] The present embodiment relates to a method for preparing a reinforced and toughened polylactic acid, comprising the following steps:
[0066] S1 Preparation of polylactic acid oligomer modified with resin microspheres
[0067] a) taking a monomer, namely L-lactide, an initiator, namely xylenol-formaldehyde resin microspheres, and a catalyst, namely stannous octoate, and melting and mixing them at 100° C. to obtain a mixed system, wherein the molar ratio of the alcohol hydroxyl group in the initiator to the lactide monomer is 5:100, and the molar ratio of stannous octoate to the lactide monomer is about 3:1000;
[0068] b) subjecting the mixed system obtained in step a) to a vacuum-nitrogen filling treatment for 3 cycles, and then reacting in an oil bath at 115° C. for 36 hours under a nitrogen atmosphere and magnetic stirring to obtain a crude product;
[0069] c) cooling the crude product obtained in step b), dissolving it in dichloromethane, purifying it by precipitation with icy methanol, and vacuum drying it at 40° C. for 48 hours to obtain a polylactic acid oligomer modified with resin microspheres;
[0070] S2 weighs the raw materials according to the following weight percentages: 15% of the polylactic acid oligomer modified with the resin microspheres obtained in step S1 and 85% of commercial polylactic acid;
[0071] S3 takes the resin microsphere modified polylactic acid oligomer and commercial polylactic acid weighed in S2, vacuum-dries them at 80°C for 18h, mixes and stirs them evenly, and adds them into a preheated torque rheometer for melt mixing, the mixing temperature is 180°C, the mixing speed is 40r / min, the mixing time is 10min, and the mixture is cooled and pelletized to obtain modified polylactic acid masterbatch;
[0072] S4: Processing the polylactic acid masterbatch obtained in step S3 in an injection molding machine with a melting temperature of 190° C. to obtain a polylactic acid composite material.
[0073] Example 5
[0074] The present embodiment relates to a method for preparing a reinforced and toughened polylactic acid, comprising the following steps:
[0075] S1 Preparation of polylactic acid oligomer modified with resin microspheres
[0076] a) taking a monomer, namely L-lactide, an initiator, namely catechin-formaldehyde resin microspheres, and a catalyst, namely stannous octoate, and melting and mixing them at 110° C. to obtain a mixed system, wherein the molar ratio of the alcohol hydroxyl group in the initiator to the lactide monomer is 5:100, and the molar ratio of stannous octoate to the lactide monomer is about 3:1000;
[0077] b) subjecting the mixed system obtained in step a) to a vacuum-filling nitrogen treatment for 3 cycles, and then reacting in an oil bath at 130° C. under a nitrogen atmosphere and magnetic stirring for 12 h to obtain a crude product;
[0078] c) cooling the crude product obtained in step b), dissolving it in dichloromethane, purifying it by precipitation with icy methanol, and vacuum drying it at 50° C. for 24 hours to obtain a polylactic acid oligomer modified with resin microspheres;
[0079] S2 weighs the raw materials according to the following weight percentages: 15% of the polylactic acid oligomer modified with the resin microspheres obtained in step S1 and 85% of commercial polylactic acid;
[0080] S3 takes the resin microsphere-modified polylactic acid oligomer and commercial polylactic acid weighed in S2, and vacuum dries them at 80°C for 18 hours respectively, mixes them, stirs them evenly, dissolves them in dichloromethane, and after mixing them evenly, casts them into a glass mold, and evaporates them in vacuum at 40°C for 24 hours to obtain a polylactic acid composite material.
[0081] Example 6
[0082] The present embodiment relates to a method for preparing a reinforced and toughened polylactic acid, comprising the following steps:
[0083] S1 Preparation of polylactic acid oligomer modified with resin microspheres
[0084] a) taking a monomer, i.e., dextrorotatory lactide, an initiator, i.e., gallic acid-formaldehyde resin microspheres, and a catalyst, i.e., stannous octoate, and melting and mixing them at 120° C. to obtain a mixed system, wherein the molar ratio of the alcohol hydroxyl group in the initiator to the lactide monomer is 1:100, and the molar ratio of stannous octoate to the lactide monomer is about 3:1000;
[0085] b) subjecting the mixed system obtained in step a) to a vacuum-nitrogen filling treatment for 3 cycles, and then reacting in an oil bath at 120° C. for 36 hours under a nitrogen atmosphere and magnetic stirring to obtain a crude product;
[0086] c) cooling the crude product obtained in step b), dissolving it in dichloromethane, purifying it by precipitation with ice methanol, and vacuum drying it at 40° C. for 24 hours to obtain a polylactic acid oligomer modified with resin microspheres;
[0087] S2 weighs the raw materials according to the following weight percentages: 15% of the polylactic acid oligomer modified with the resin microspheres obtained in step S1 and 85% of commercial polylactic acid;
[0088] S3 takes the resin microsphere-modified polylactic acid oligomer and commercial polylactic acid weighed in S2, and vacuum dries them at 80°C for 18 hours respectively, mixes them, stirs them evenly, dissolves them in dichloromethane, and after mixing them evenly, casts them into a glass mold, and evaporates them in vacuum at 40°C for 24 hours to obtain a polylactic acid composite material.
Claims
1. A polylactic acid oligomer modified with resin microspheres, characterized in that: The preparation method is: a) taking lactide monomer, resin microsphere initiator and catalyst and melting them at 100-120° C. to obtain a mixture, wherein the molar ratio of alcohol hydroxyl group in the resin microsphere initiator to lactide monomer is 1-15:100; b) reacting the mixture obtained in step a) at 115-130° C. under an inert gas atmosphere and stirring to obtain a crude product; c) cooling, purifying and drying the crude product obtained in step b) to obtain a polylactic acid oligomer modified with resin microspheres; The resin microspheres are phenolic resin microspheres containing a plurality of alcohol hydroxyl initiating groups.
2. The polylactic acid oligomer modified with resin microspheres according to claim 1, characterized in that: The degree of polymerization in the branched chain of the polylactic acid oligomer is 63-91, and the corresponding single-arm number average molecular weight of the polylactic acid oligomer is 1000-10000 g / mol.
3. The polylactic acid oligomer modified with resin microspheres according to claim 1, characterized in that: Step b), react at 115-130°C for 12-48h.
4. The polylactic acid oligomer modified with resin microspheres according to claim 1, characterized in that: Step c), cooling the crude product obtained in step b), dissolving it in dichloromethane, purifying it by precipitation with icy methanol, and drying it in vacuum at 40-50° C. for 24-48 hours.
5. The polylactic acid oligomer modified with resin microspheres according to claim 1, characterized in that: The resin microspheres are phenolic resin microspheres synthesized by phenolic compounds and formaldehyde or hexamethylenetetramine through phenolic reaction.
6. The polylactic acid oligomer modified with resin microspheres according to claim 1, characterized in that: The resin microspheres are one or more of xylenol-formaldehyde resin microspheres, catechin-formaldehyde resin microspheres, gallic acid-formaldehyde resin microspheres, phenol-formaldehyde resin microspheres, catechol-formaldehyde resin microspheres and resorcinol-formaldehyde resin microspheres.
7. The resin microsphere-modified polylactic acid oligomer according to claim 1, characterized in that: The lactide monomer is any one of L-lactide, D-lactide and meso-lactide.
8. The resin microsphere-modified polylactic acid oligomer according to claim 1, characterized in that: The catalyst is any one of 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD), stannous octoate, stannous chloride, cycloalkoxytin, lithium chloride, and aluminum isopropoxide, and the molar ratio of the catalyst to the lactide monomer is 1-5:1000.
9. A polylactic acid composite material, characterized in that: The invention is prepared by blending 1-15% by mass of the polylactic acid oligomer modified by the resin microspheres according to claims 1-8 and 85-99% of commercial polylactic acid.
10. The polylactic acid composite material according to claim 9, characterized in that: The number average molecular weight of the commercial polylactic acid is 8-15×10 4 g / mol.
Citation Information
Patent Citations
Research method for preparing 1,2-propylene glycol by hydrogenating ethyl lactate
CN110028387A
High-strength acrylate cross-linked microsphere grafted modified polylactic acid and preparation method thereof
CN111534069A
Nano sponge structure gel material, preparation method and application thereof, and water quality detection method
CN114989477A
Tri-block copolymers and NANO-fibrous gelling microspheres including the same