Preparation method of high-performance hyperbranched concrete modifier based on controllable degradation of waste resin

The controllable degradation of waste epoxy resin forms a hyperbranched structure to address the limitations of existing modifiers, enhancing concrete fluidity and strength while reducing carbon emissions.

CN119081230AActive Publication Date: 2024-12-06SICHUAN UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411186096.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Existing hyperbranched concrete modifiers face issues of low molecular weight, uncontrollable structure, high manufacturing costs, and high carbon emissions, limiting their practical application in high-performance concrete.

Method used

A method involving the controllable degradation of waste epoxy resin to form a hyperbranched structure using polyamines and boric acid, adjusting molecular weight and branched modification to enhance concrete fluidity and strength.

Benefits of technology

The method results in a high-performance concrete modifier with adjustable properties, improving fluidity and mechanical strength, and reducing carbon footprint by utilizing waste materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081230A_ABST
    Figure CN119081230A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-performance hyperbranched concrete modifier based on controllable degradation of waste resin, particularly relates to the field of concrete modifiers, and belongs to low-carbon high-strength concrete materials. Waste epoxy resin is subjected to swelling pretreatment in a good solvent, so that the reaction activity is improved, the waste epoxy resin is used as a catalyst for next-step reaction, and in the presence of polyamine, partial degradation of the polymer is realized through low-temperature swelling treatment-high-temperature partial degradation. The construction of a hyperbranched structure on the surface of the waste is realized by utilizing a chemical reaction of amino and hydroxyl on the surface of a part of degradation products and polyfunctional boric acid hydroxyl, and the water reducing rate of the prepared concrete high-performance modifier is greater than or equal to 30%. The method for constructing the partially degraded hyperbranched structure is mild in condition, simple in step and low in cost, the key problems that a cement high-performance modifier is complex in synthesis, high in carbon emission and the like are solved, the mechanical property of concrete is greatly improved through products, and the method is widely applied to the field of low-carbon high-strength concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete modifiers, and particularly relates to a method for preparing a high-performance hyperbranched concrete modifier based on controllable degradation of waste resin. Background Art

[0002] As the most important building material, concrete is widely used in civil engineering, water conservancy and national defense construction due to its excellent mechanical properties and durability. In the Outline for Building a Quality Power Country issued by my country in 2023, it is clearly proposed to promote the application of high-performance concrete as a green building material, and to comprehensively utilize solid waste resources to achieve green carbon reduction.

[0003] Modifiers represented by water reducers are essential components of modern high-performance concrete because they can improve the mechanical properties of concrete while improving the workability and fluidity of concrete. Among them, hyperbranched modifiers have attracted widespread attention due to their excellent water-reducing ability brought by their nearly spherical three-dimensional molecular shape and high-density reactive groups. However, hyperbranched modifiers usually face bottleneck problems such as low molecular weight, uncontrollable structure, product value that cannot cover manufacturing costs, and high carbon emissions, making them difficult to be applied in practice.

[0004] Therefore, developing hyperbranched modifiers from waste materials to achieve efficient water reduction of cement and effectively enhance its mechanical properties is of great significance to the development of the cement industry. Summary of the invention

[0005] In view of the above problems, the present invention provides a method for preparing a high-performance hyperbranched concrete modifier based on the controllable degradation of waste resin, aiming to solve the technical problems encountered in the application of existing high-performance concrete modifiers. Its characteristics are:

[0006] The waste epoxy resin is pre-treated by swelling in a good solvent to improve its reaction activity and act as a catalyst for the next reaction. In the presence of polyamines, the above polymer is partially degraded by low-temperature swelling treatment-high-temperature partial degradation. The strong interaction between the amino and hydroxyl groups on the surface of the partially degraded product and the boric acid hydroxyl structure is used to construct a hyperbranched structure on the surface of the waste. The polyhydroxyl and polyamino structures brought by the hyperbranched structure allow the modifier to form a solvation film with water molecules, thereby effectively reducing the sliding resistance of cement particles, thereby improving the fluidity of concrete.

[0007] Based on the three-branched structure and electron-deficient effect of the boron element, by controlling the polyamine, type and group density, the molecular weight and branched modification of the obtained partially degraded waste can be adjusted, which can effectively improve the fluidity required for concrete construction and greatly improve the strength of concrete.

[0008] In order to solve the above technical problems, the present invention is achieved by the following technical means: a method for preparing a high-performance hyperbranched concrete modifier based on controllable degradation of waste resin, comprising the following steps:

[0009] (1) maintaining a certain stirring rate in a good solvent, stirring the waste epoxy resin at room temperature for 24-72 hours, and drying after the polymer is completely swollen to obtain the pretreated waste epoxy resin;

[0010] (2) adding the pretreated waste epoxy resin to the polyamine, heating and stirring for 2-6 hours, and stopping the reaction after the solution viscosity increases to 500-1000 Pa·s;

[0011] (3) The above solution was added dropwise to 500 ml of ethanol, and ultrasonicated at 200-600 W for 1 h at room temperature, and then centrifuged at 9000 r / min for 5 min;

[0012] (4) Add the precipitate after centrifugation to N,N-dimethylformamide and stir until dissolved, then add boric acid, stir at room temperature for 4-8 hours, then heat to 80°C, dry completely, and cool to obtain a high-performance hyperbranched concrete modifier.

[0013] Furthermore, the good solvent is at least one of dichloromethane, chloroform, acetic acid, acetone, and dimethyl carbonate.

[0014] Furthermore, the polyamine is at least one of ethylenediamine, diethylenetriamine and triethylenetetramine.

[0015] The present invention also discloses a high-performance hyperbranched concrete modifier based on controllable degradation of waste resin, which is prepared according to any of the above preparation methods.

[0016] The present invention also discloses an application of the high-performance hyperbranched concrete modifier based on the controllable degradation of waste resin in the preparation of low-carbon high-strength concrete.

[0017] Furthermore, the high-performance hyperbranched concrete modifier is mixed with cement aggregate in a mass ratio of 1:100 to obtain low-carbon high-strength concrete.

[0018] Compared with the prior art, the waste epoxy resin controllable degradation and hyperbranched modification to prepare the concrete modifier described in this application has the following characteristics:

[0019] 1. The present invention prepares a high-performance concrete modifier based on waste-derived epoxy resin materials, thereby avoiding the problems of high cost and excessive carbon emissions caused by the complex synthesis of high-performance modifiers.

[0020] 2. The present invention controls the polyamine, type and group density and reaction temperature during degradation, so that the molecular weight of the partially degraded waste and the branched modified group density are adjustable, and can be applied to concrete of different grades and types.

[0021] 3. The method for partial degradation and hyperbranching of discarded materials established by the present invention has simple steps and controllable product structure. The water reduction rate of the high-performance modifier is ≥30%, and the mechanical properties of concrete are greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is the chemical change process in the material preparation method described in Example 1 of the present application.

[0023] Figure 2 This is a GPC chart of the molecular weight of the epoxy resin after partial degradation described in Example 1 of the present application.

[0024] Figure 3 This is a Raman spectrum of the hydration rate of the concrete before and after the modifier is added to Example 1 of the present application.

[0025] Figure 4 It is the flexural strength and compressive strength of the concrete described in Example 1 of the present application. DETAILED DESCRIPTION

[0026] The present invention is specifically described below through examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments to the present invention based on the above content.

[0027] Embodiment 1:

[0028] Take 30g of waste anhydride cured epoxy resin and 100ml of dichloromethane and stir at a stirring rate of 500r / min for 24h until the polymer is completely swollen, then dry and collect for later use. Accurately weigh 80ml of diethylenetriamine, slowly add the swollen epoxy resin, stir at a speed of 500r / min and heat to 160℃, and cool down to terminate the reaction after 2h. Add the obtained high viscosity solution to 500ml of ethanol, and ultrasonicate at 200W power for 1h at room temperature, and then centrifuge at a speed of 9000r / min for 5min. Add the precipitate after centrifugation to 100ml N,N-dimethylformamide and stir for 20min until dissolved. Add 5g of boric acid to the above solution, stir at room temperature for 4-8h, then heat to 80℃, completely dry after 4h, and cool to obtain a high-performance hyperbranched concrete modifier.

[0029] The obtained modifier is mixed with cement aggregate in a ratio of 1:100, the cement hydration rate is greatly accelerated, the water reduction rate is ≥30%, the flexural strength of concrete is increased by more than 15%, and the compressive strength is increased by more than 20%. Figure 2 This is the molecular weight GPC diagram of the epoxy resin after partial degradation described in Example 1 of the present application. Figure 2 The results show that the molecular weight of the degradation product is 2034 and the molecular weight distribution index is 1.878, indicating that the epoxy resin has been successfully degraded in a controlled manner. It can be seen that the method proposed in this application can achieve the controllable degradation of the epoxy resin. Figure 3 is the Raman spectrum of the hydration rate of the concrete before and after adding the modifier in Example 1 of the present application. Figure 3 The results show that the corresponding peak intensity of cement hydrated calcium silicate increases significantly after adding the modifier. It can be seen that the hydration rate of cement is greatly improved after adding the modifier. Figure 4 is the flexural strength and compressive strength of the concrete described in Example 1 of the present application, according to Figure 4 The results show that after adding the modifier, the flexural strength of the concrete is increased by more than 15%, and the compressive strength is increased by more than 20%. It can be seen that the method proposed in this application can achieve the improvement of the flexural strength and compressive strength of concrete.

[0030] Embodiment 2:

[0031] Take 30g of waste anhydride cured epoxy resin and 100ml of dichloromethane and stir at a stirring rate of 500r / min for 24h until the polymer is completely swollen, then dry and collect for later use. Accurately weigh 80ml of diethylenetriamine, slowly add the swollen epoxy resin, stir at a speed of 500r / min and heat to 160℃, and cool down to terminate the reaction after 2h. Add the obtained high viscosity solution to 500ml of ethanol, and ultrasonicate at 600W power for 1h at room temperature, and centrifuge at a speed of 9000r / min for 5min. Add the precipitate after centrifugation to 100ml N, N-dimethylformamide and stir for 20min until dissolved. Add 5g of boric acid to the above solution, stir at room temperature for 4-8h, then heat to 80℃, 4h until completely dried, and cool to obtain a high-performance hyperbranched concrete modifier.

[0032] The obtained modifier is mixed with cement aggregate in a ratio of 1:100, the cement hydration rate is greatly accelerated, the water reduction rate is ≥20%, the flexural strength of concrete is increased by more than 10%, and the compressive strength is increased by more than 15%.

[0033] The above are only preferred embodiments of the present application, and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A method for preparing a high-performance hyperbranched concrete modifier based on controllable degradation of waste resin, comprising: (1) stirring the waste epoxy resin in a good solvent, drying after the polymer is completely swollen, and obtaining the pretreated waste epoxy resin; (2) adding the pretreated waste epoxy resin to the polyamine, heating it, and stirring it thoroughly for 2-6 hours, and stopping the reaction according to the change in solution viscosity; (3) adding the solution obtained in step (2) dropwise into 500 ml of ethanol, ultrasonically treating at room temperature, and then centrifuging; (4) Add the precipitate obtained after centrifugation in step (3) into 100 ml of N,N-dimethylformamide and stir until dissolved, then add boric acid and stir, heat and dry, and then cool to obtain a high-performance hyperbranched concrete modifier.

2. The preparation method according to claim 1, wherein: The mass volume ratio of the waste epoxy resin to the good solvent in step (1) is 30g:100ml.

3. The preparation method according to claim 1, wherein: The stirring speed in step (1) is 500 r / min and the stirring time is 24 h; The good solvent is at least one of dichloromethane, chloroform, acetic acid, acetone and dimethyl carbonate.

4. The preparation method according to claim 1, wherein: The polyamine in step (2) is at least one of ethylenediamine, diethylenetriamine and triethylenetetramine; The amount of the polyamine used is 80 ml.

5. The preparation method according to claim 1, wherein: The heating in step (2) is to raise the temperature to 160-180° C. The end point of stopping the reaction is: reacting until the solution viscosity rises to 500-1000 Pa·s.

6. The preparation method according to claim 1, wherein: The ultrasonic treatment power in step (3) is 200-600W, and the ultrasonic treatment time is 1h; The centrifugal speed is 9000 r / min, and the centrifugal time is 5 min.

7. The preparation method according to claim 1, wherein: The stirring time in step (4) is 4-8h; The heating and drying temperature is 80°C.

8. A controllably degradable high-performance hyperbranched concrete modifier based on waste resin prepared according to the preparation method of any one of claims 1 to 7.

9. Use of the high-performance hyperbranched concrete modifier based on controlled degradation of waste resin according to claim 8 in the preparation of low-carbon high-strength concrete.

10. The use according to claim 9, wherein: The mass ratio of the waste resin-based controllable degradation high-performance hyperbranched concrete modifier to cement aggregate is 1:100, so as to obtain low-carbon high-strength concrete.

Citation Information

Patent Citations

  • Environment-friendly concrete water reducing agent and preparation method thereof

    CN112194407A

  • Concrete pumping agent and preparation method thereof

    CN113105146A

  • Branched-structure graphene oxide-polycarboxylate superplasticizer composite material and preparation method thereof

    CN117658515A

  • Epoxy intumescent fire retardant coating with low glass transition temperature and high temperature resistance

    CN117820603A

  • Self-healing polymer-modified cements for ambient temperature applications

    US20230109371A1