Refractory material, preparation method thereof and application of refractory material in telescopic rod

By adjusting the mass ratio of wollastonite fibers, wollastonite powder and aralkylphenol-type self-flame retardant epoxy resin, and modifying wollastonite fibers and wollastonite powder, the refractory resistance of ceramicized polyolefin materials and The problem of insufficient deformation resistance has achieved significant improvements in fire resistance and deformation resistance, and broadened its application scope.

CN119081256APending Publication Date: 2024-12-06HEBEI JUMAI NEW MATERIALS TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410702185.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-01
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing ceramicized polyolefin refractory materials have material deformation problems caused by insufficient strength while improving their refractory properties, which limits their application in different environments.

Method used

The mass ratio of wollastonite fiber, wollastonite powder and aralkylphenol-type self-flame-retardant epoxy resin is adjusted, and wollastonite fiber and wollastonite powder are modified by tetradecanediic acid, combined with flux and lubricant and anti-aging agent, a refractory material is prepared, and the refractory and deformation resistance of the material are improved through the extrusion molding process.

Benefits of technology

It significantly improves the refractory resistance and deformation resistance of refractory materials, and broadens its application range in different environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081256A_ABST
    Figure CN119081256A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of refractory materials, and provides a refractory material and a preparation method and application thereof in a telescopic rod, the refractory material comprises the following components by weight: 80-90 parts of polyolefin, 30-50 parts of a filler, 10-15 parts of a fluxing agent, 2-4 parts of a lubricant, and 0.5-1 part of an anti-aging agent; the filler is composed of wollastonite fibers, pyrophyllite powder and aralkyl phenol type self-flame-retardant epoxy resin. According to the technical scheme, the problem that a refractory material in the prior art is poor in deformation resistance and fire resistance is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of refractory materials, and in particular to a refractory material and a preparation method thereof and an application of the refractory material in a telescopic rod. Background Art

[0002] Polyolefins occupy an important position in all industrial links, but the flammability of polymer materials themselves limits the expansion of their application scope. In order to improve the fire resistance of polyolefin materials, new refractory materials, ceramic polyolefins, have begun to be widely studied and applied to various fields that require fire resistance. However, while the existing ceramic polyolefin refractory materials have improved their fire resistance, they still have the problem of material deformation caused by insufficient strength, which makes it impossible to further apply ceramic polyolefin materials in some occasions. Therefore, it is urgent to develop a polyolefin refractory material with excellent deformation resistance and fire resistance to broaden the application of refractory materials in different environments. Summary of the invention

[0003] The present invention provides a refractory material and a preparation method thereof and application of the refractory material in a telescopic rod, thereby solving the problems of poor deformation resistance and fire resistance of the refractory material in the related art.

[0004] The technical solution of the present invention is as follows: The present invention provides a refractory material, comprising the following components in parts by weight: 80-90 parts of polyolefin, 30-50 parts of filler, 10-15 parts of flux, 2-4 parts of lubricant, and 0.5-1 part of antioxidant; The filler consists of wollastonite fiber, pyrophyllite powder and aralkylphenol type self-flame retardant epoxy resin.

[0005] As a further technical solution, the mass ratio of the wollastonite fiber, pyrophyllite powder and aralkylphenol type self-flame retardant epoxy resin is 4:1:1-5.

[0006] In the present invention, the mass ratio of wollastonite fiber, pyrophyllite powder and aralkylphenol type self-flame retardant epoxy resin is adjusted to 4:1:1-5, thereby further improving the fire resistance and deformation resistance of the refractory material.

[0007] As a further technical solution, the mass ratio of the wollastonite fiber, pyrophyllite powder and aralkylphenol type self-flame retardant epoxy resin is 4:1:2-3.

[0008] In the present invention, the mass ratio of wollastonite fiber, pyrophyllite powder and aralkylphenol type self-flame retardant epoxy resin is limited to 4:1:2-3, thereby further improving the deformation resistance of the refractory material.

[0009] As a further technical solution, the wollastonite fiber and pyrophyllite powder in the filler are modified by tetradecanedioic acid.

[0010] As a further technical solution, the modified preparation method comprises the following steps: mixing wollastonite fiber, pyrophyllite powder and tetradecanedioic acid in a solvent and removing the solvent to obtain the modified fiber.

[0011] As a further technical solution, the mass ratio of the total mass of the wollastonite fiber and pyrophyllite powder to tetradecanedioic acid is 16-20:1; the volume ratio of the total mass of the wollastonite fiber and pyrophyllite powder to the solvent is 1g:1.2-1.5mL.

[0012] As a further technical solution, the mixing temperature is 95-105° C. and the mixing time is 3.5-4.5 hours.

[0013] In the present invention, tetradecanedioic acid is used to modify wollastonite fiber and pyrophyllite powder, thereby further improving the deformation resistance of the refractory material.

[0014] As a further technical solution, the polyolefin is one or more of chlorinated polyethylene, polyethylene and chlorosulfonated polyethylene; the lubricant is one of stearic acid and polyethylene wax; the antioxidant is an amine antioxidant or a phenolic antioxidant; and the flux is a mixture of glass powder and zinc borate.

[0015] The present invention also provides a method for preparing the refractory material, comprising the following steps: The components of the refractory material are mixed and then extruded to obtain the refractory material.

[0016] The present invention also proposes the use of the refractory material or the refractory material prepared by the preparation method in a telescopic rod.

[0017] The working principle and beneficial effects of the present invention are: In the present invention, wollastonite fiber and pyrophyllite powder are vitrified and flame retardant is coordinated with aralkylphenol type self-flame retardant epoxy resin, thereby significantly improving the fire resistance and deformation resistance of the refractory material. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0019] Figure 1 This is a schematic diagram of a telescopic rod made of refractory material according to Example 3 of the present invention. DETAILED DESCRIPTION

[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] In the following embodiments and comparative examples, the model of polyethylene is PE-100; the model of chlorinated polyethylene is CPE-135A; the model of arylalkylphenol self-flame retardant epoxy resin is PXNE2000, purchased from Hunan Jiashengde Materials Technology Co., Ltd.; the average length of wollastonite fiber is 10 μm; and the average particle size of pyrophyllite powder is 20 μm.

[0022] Example 1 A refractory material, comprising the following components in parts by weight: 60 parts of polyethylene, 20 parts of chlorinated polyethylene, 30 parts of filler, 5 parts of glass powder, 5 parts of zinc borate, 2 parts of polyethylene wax, and 0.5 parts of antioxidant 2246; wherein the filler is composed of wollastonite fiber, pyrophyllite powder and aralkylphenol type self-flame retardant epoxy resin in a mass ratio of 2:1:2; The method for preparing a refractory material comprises the following steps: The components of the refractory material are mixed and then extruded to obtain the refractory material.

[0023] Example 2 A refractory material, comprising the following components in parts by weight: 90 parts of chlorinated polyethylene, 50 parts of filler, 7.5 parts of glass powder, 7.5 parts of zinc borate, 4 parts of polyethylene wax, and 1 part of antioxidant 2246; wherein the filler is composed of wollastonite fiber, pyrophyllite powder, and aralkylphenol type self-flame retardant epoxy resin in a mass ratio of 2:1:2; The method for preparing a refractory material comprises the following steps: The components of the refractory material are mixed and then extruded to obtain the refractory material.

[0024] Example 3 A refractory material, comprising the following components in parts by weight: 60 parts of polyethylene, 25 parts of chlorinated polyethylene, 42 parts of filler, 6 parts of glass powder, 6 parts of zinc borate, 3 parts of polyethylene wax, and 1 part of antioxidant 2246; wherein the filler is composed of wollastonite fiber, pyrophyllite powder and aralkylphenol type self-flame retardant epoxy resin in a mass ratio of 2:1:2; The method for preparing a refractory material comprises the following steps: The components of the refractory material are mixed and then extruded to obtain the refractory material.

[0025] Example 4 The only difference between this embodiment and embodiment 3 is that the filler is composed of wollastonite fiber, pyrophyllite powder and aralkylphenol type self-flame retardant epoxy resin in a mass ratio of 6:1:1.

[0026] Example 5 The only difference between this embodiment and embodiment 3 is that the filler is composed of wollastonite fiber, pyrophyllite powder and aralkylphenol type self-flame retardant epoxy resin in a mass ratio of 4:1:1.

[0027] Example 6 The only difference between this embodiment and embodiment 3 is that the filler is composed of wollastonite fiber, pyrophyllite powder and aralkylphenol type self-flame retardant epoxy resin in a mass ratio of 4:1:5.

[0028] Example 7 The only difference between this embodiment and embodiment 3 is that the filler is composed of wollastonite fiber, pyrophyllite powder and aralkylphenol type self-flame retardant epoxy resin in a mass ratio of 4:1:2.

[0029] Example 8 The only difference between this embodiment and embodiment 3 is that the filler is composed of wollastonite fiber, pyrophyllite powder and aralkylphenol type self-flame retardant epoxy resin in a mass ratio of 4:1:3.

[0030] Example 9 The only difference between this embodiment and embodiment 8 is that the wollastonite fiber and pyrophyllite powder in the filler are modified by octadecanoic acid; the modified preparation method comprises the following steps: mixing the wollastonite fiber, pyrophyllite powder and octadecanoic acid in toluene at 95°C for 4.5 hours, and removing the toluene to obtain the product; wherein the mass ratio of the total mass of the wollastonite fiber and pyrophyllite powder to octadecanoic acid is 20:1; and the volume ratio of the total mass of the wollastonite fiber and pyrophyllite powder to the solvent is 1 g:1.5 mL.

[0031] Example 10 The only difference between this embodiment and embodiment 8 is that the wollastonite fiber and pyrophyllite powder in the filler are modified by tetradecanedioic acid; the modified preparation method comprises the following steps: mixing the wollastonite fiber, pyrophyllite powder and tetradecanedioic acid in toluene at 95°C for 4.5 hours, and removing the toluene to obtain the product; wherein the mass ratio of the total mass of the wollastonite fiber and pyrophyllite powder to tetradecanedioic acid is 20:1; and the volume ratio of the total mass of the wollastonite fiber and pyrophyllite powder to the solvent is 1 g:1.5 mL.

[0032] Embodiment 11 The only difference between this embodiment and embodiment 8 is that the wollastonite fiber and pyrophyllite powder in the filler are modified by tetradecanedioic acid; the modified preparation method comprises the following steps: mixing the wollastonite fiber, pyrophyllite powder and tetradecanedioic acid in toluene at 105°C for 3.5 hours, and removing the toluene to obtain the product; wherein the mass ratio of the total mass of the wollastonite fiber and pyrophyllite powder to tetradecanedioic acid is 16:1; and the volume ratio of the total mass of the wollastonite fiber and pyrophyllite powder to the solvent is 1g:1.2mL.

[0033] Comparative Example 1 The only difference between this comparative example and Example 3 is that the filler consists of wollastonite fiber and aralkylphenol type self-flame retardant epoxy resin in a mass ratio of 1:1.

[0034] Comparative Example 2 The only difference between this comparative example and Example 3 is that the filler consists of wollastonite fiber and pyrophyllite powder in a mass ratio of 2:1.

[0035] Comparative Example 3 The difference between this comparative example and Example 3 is that the filler is composed of pyrophyllite powder and aralkylphenol type self-flame retardant epoxy resin in a mass ratio of 1:2.

[0036] Application Examples The telescopic rod made of the refractory material of Example 3 is as follows Figure 1 shown.

[0037] performance The performance tests were performed on the refractory materials prepared in Examples 1 to 11 and Comparative Examples 1 to 3 respectively: Deformation resistance: Notched impact strength test was carried out according to the standard GB / T 1843-2008 "Determination of Izod Impact Strength of Plastics", the notch type was A type, and the notch size was r N =0.25±0.5mm, b N =8.0±0.2mm; each sample is measured three times in parallel and the average value is taken, and the result is retained to one decimal place; where r N is the notch bottom radius, b N is the reserved width of the gap; Fire resistance: The vertical burning grade test is carried out in accordance with the experimental method B-vertical burning test in the standard GB / T 2408-2021 "Horizontal and vertical methods for determination of combustion performance of plastics".

[0038] The test results are shown in Table 1.

[0039] Table 1 Fire resistance and deformation resistance test results

[0040] By comparing the data of Examples 1 to 11 and Comparative Examples 1 to 3, it is found that compared with Comparative Examples 1 to 3, the vertical combustion level and tensile strength of the refractory materials prepared in Examples 1 to 11 are higher, indicating that the synergistic use of wollastonite fiber, pyrophyllite powder vitrification and aromatic alkylphenol type self-flame retardant epoxy resin can significantly improve the fire resistance and deformation resistance of the refractory materials.

[0041] By comparing the data of Examples 3 to 8, it is found that compared with Examples 3 to 4, the vertical combustion level and tensile strength of the refractory materials prepared in Examples 5 to 6 are higher, indicating that by adjusting the mass ratio of wollastonite fiber, pyrophyllite powder and arylalkylphenol type self-flame retardant epoxy resin to 4:1:1 to 5, the fire resistance and deformation resistance of the refractory materials are further improved; compared with Examples 5 to 6, the tensile strength of the refractory materials prepared in Examples 7 to 8 is higher, indicating that by limiting the mass ratio of wollastonite fiber, pyrophyllite powder and arylalkylphenol type self-flame retardant epoxy resin to 4:1:2 to 3, the deformation resistance of the refractory materials can be further improved.

[0042] By comparing the data of Examples 8 to 11, it is found that compared with Examples 8 to 9, the tensile strength of the refractory materials prepared in Examples 10 to 11 is higher, indicating that the modification of wollastonite fiber and pyrophyllite powder by tetradecanedioic acid can further improve the deformation resistance of the refractory materials.

[0043] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A refractory material, characterized in that: The invention comprises the following components in parts by weight: 80-90 parts of polyolefin, 30-50 parts of filler, 10-15 parts of flux, 2-4 parts of lubricant, and 0.5-1 part of antioxidant; The filler consists of wollastonite fiber, pyrophyllite powder and aralkylphenol type self-flame retardant epoxy resin.

2. A refractory material according to claim 1, characterized in that: The mass ratio of the wollastonite fiber, the pyrophyllite powder and the aralkylphenol type self-flame retardant epoxy resin is 4:1:1-5.

3. A refractory material according to claim 2, characterized in that: The mass ratio of the wollastonite fiber, the pyrophyllite powder and the aralkylphenol type self-flame retardant epoxy resin is 4:1:2-3.

4. A refractory material according to claim 1, characterized in that: The wollastonite fiber and pyrophyllite powder in the filler are obtained by modification of tetradecanedioic acid.

5. A refractory material according to claim 4, characterized in that: The modified preparation method comprises the following steps: mixing wollastonite fiber, pyrophyllite powder and tetradecanedioic acid in a solvent and removing the solvent to obtain the modified fiber.

6. A refractory material according to claim 5, characterized in that: The mass ratio of the total mass of the wollastonite fiber and the pyrophyllite powder to tetradecanedioic acid is 16-20:1; the volume ratio of the total mass of the wollastonite fiber and the pyrophyllite powder to the solvent is 1g:1.2-1.5mL.

7. A refractory material according to claim 5, characterized in that: The mixing temperature is 95-105° C. and the mixing time is 3.5-4.5 hours.

8. A refractory material according to claim 1, characterized in that: The polyolefin is one or more of chlorinated polyethylene, polyethylene and chlorosulfonated polyethylene; the lubricant is one of stearic acid and polyethylene wax; the antioxidant is an amine antioxidant or a phenolic antioxidant; and the flux is a mixture of glass powder and zinc borate.

9. The method for preparing a refractory material according to any one of claims 1 to 8, characterized in that: The following steps are involved: The components of the refractory material are mixed and then extruded to obtain the refractory material.

10. Use of the refractory material according to any one of claims 1 to 8 or the refractory material prepared by the preparation method according to claim 9 in a telescopic rod.