High-toughness antioxidant flame-retardant color master batch and preparation method thereof
By using a combination of inorganic pigments, ethylene-vinyl acetate copolymers and layered double hydroxides, the problem of insufficient toughness, antioxidant and flame retardant properties of masterbatches is solved, and a high-toughness, antioxidant and flame retardant color is prepared. Masterbatch, suitable for high-end materials applications, meets the requirements for flame retardant performance in high-end fields.
Patent Information
- Application Number
- CN202411402062.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing masterbatch has shortcomings in toughness, oxidation resistance and flame retardant properties, which limits its application in high-end fields, especially in the fields of electronics, automotive, aerospace, etc.
High toughness and antioxidant are prepared by high-speed mixing and segmented twin screw extruder granulation process using inorganic pigments, ethylene-vinyl acetate copolymers, layered double hydroxides, talc powder, dispersants and antioxidants. The flame-retardant masterbatch uses the flexibility of the ethylene-vinyl acetate copolymer and the nano-size effect and antioxidant properties of the layered double hydroxide to form a synergistic flame-retardant effect.
It improves the toughness and flame retardant properties of the masterbatch, so that it maintains good performance when the material is repeatedly bending or deformed, has strong oxidation resistance and good flame retardant properties, and is suitable for high-end materials applications.
Smart Images

Figure BDA0005075555060000051 
Figure BDA0005075555060000061 
Figure BDA0005075555060000071
Abstract
Description
Technical Field
[0001] The invention relates to the field of masterbatch materials, and in particular to a high-toughness, anti-oxidation and flame-retardant masterbatch and a preparation method thereof. Background Art
[0002] As a colorant for polymer materials, masterbatch has been widely used in the fields of plastics, rubber, fiber, etc. It is a granular substance composed of pigments, carrier resins and various additives. By mixing with the matrix material, it can give the product specific color and performance. However, the masterbatch on the market still has some shortcomings in toughness, anti-oxidation and flame retardancy, which limits its application in some high-end fields. The development of masterbatch can be traced back to the 1950s, when it was mainly used for coloring plastics. With the rapid development of the plastics industry, the variety and performance of masterbatch have been continuously improved, and the scope of application has gradually expanded. At present, masterbatch has become an indispensable colorant in the plastics, rubber, fiber and other industries. In the process of development, the technology of masterbatch has been continuously innovated. Early masterbatch was mainly prepared by a simple mixing method of pigment and carrier resin, and its performance was poor. Later, with the development of polymer material science, people began to use advanced blending, extrusion, granulation and other technologies to prepare masterbatch, which significantly improved its performance. At the same time, in order to meet the needs of different fields, people have also developed various functional masterbatches, such as flame retardant masterbatches, antistatic masterbatches, antibacterial masterbatches, etc.
[0003] The application field of masterbatch is very wide. Masterbatch is most widely used in the plastic industry. It can be used to color various plastic products, such as plastic film, plastic pipe, plastic sheet, plastic injection molded parts, plastic extruded parts, etc. Different plastic products have different performance requirements for masterbatch. For example, plastic film requires masterbatch to have good dispersibility and transparency, plastic pipe requires masterbatch to have good corrosion resistance and pressure resistance, plastic injection molded parts require masterbatch to have good fluidity and heat resistance, etc. The application of masterbatch in the rubber industry is also becoming more and more extensive. It can be used to color various rubber products, such as tires, hoses, tapes, rubber soles, etc. Compared with the plastic industry, the rubber industry has higher performance requirements for masterbatch, such as requiring masterbatch to have good heat resistance, aging resistance, oil resistance and wear resistance. The application of masterbatch in the fiber industry is mainly used for the coloring of chemical fibers, such as polyester fibers, nylon fibers, polypropylene fibers, etc. Masterbatch can make chemical fibers have bright colors and good light resistance, washability and other properties. Masterbatch can also be used for coloring in coatings, inks, papermaking and other industries, as well as in some special fields such as food packaging, pharmaceutical packaging, electronic appliances, etc.
[0004] The lack of toughness of masterbatch is a common problem, which is mainly caused by factors such as the performance of the carrier resin and the amount of pigment added. Generally speaking, the better the toughness of the carrier resin, the better the toughness of the masterbatch. However, in order to improve the color and hiding power of the masterbatch, a large amount of pigment is often needed to be added, which will reduce the toughness of the masterbatch. In addition, the high hardness of some pigments themselves will also affect the toughness of the masterbatch. Masterbatch is easily affected by oxidation during processing and use, resulting in its performance degradation. This is mainly because the carrier resin and pigment components in the masterbatch easily react with oxygen in the air to produce free radicals, thereby causing oxidative degradation. The poor flame retardant performance of the masterbatch is also a problem that needs attention. In some special fields, such as electronic appliances, automobiles, aerospace, etc., the flame retardant performance of the material is very high. If the flame retardant performance of the masterbatch is not good, it may cause the product to fail to play an effective flame retardant role in the event of a fire, thereby increasing the risk of fire.
[0005] As an important polymer material colorant, masterbatch has been widely used in the fields of plastics, rubber, fiber, etc. However, the masterbatch currently on the market still has some deficiencies in toughness, anti-oxidation and flame retardancy. In view of the problems existing in the prior art, this application aims to solve the problem of insufficient toughness, anti-oxidation and flame retardancy of masterbatch. Summary of the invention
[0006] Purpose of the invention: The purpose of the present invention is to provide a high-toughness, antioxidant and flame-retardant masterbatch and a preparation method thereof, so as to solve the problem of insufficient toughness, antioxidant and flame-retardant properties of the masterbatch.
[0007] The technical solution of the present invention:
[0008] The invention discloses a high-toughness antioxidant flame-retardant masterbatch, characterized in that the raw materials for preparing the high-toughness antioxidant flame-retardant masterbatch include: inorganic pigment, ethylene-vinyl acetate copolymer, layered double hydroxide, talcum powder, dispersant and antioxidant.
[0009] Furthermore, the raw materials for preparing the high-toughness antioxidant flame-retardant masterbatch include, by weight: 15 to 25 parts of inorganic pigment, 40 to 60 parts of ethylene-vinyl acetate copolymer, 8 to 12 parts of layered double hydroxide, 1 to 3 parts of talc, 4 to 8 parts of dispersant, and 2 to 4 parts of antioxidant.
[0010] Furthermore, the mass content of ethylene in the ethylene-vinyl acetate copolymer is 8-14% of the ethylene-vinyl acetate copolymer.
[0011] Furthermore, the layered double hydroxide is formed by reacting magnesium chloride, aluminum chloride, carbon nanotubes and sodium hydroxide.
[0012] The preparation method of the layered double hydroxide comprises the following steps:
[0013] S1: dissolving magnesium chloride and aluminum chloride in a certain amount of deionized water respectively to prepare a magnesium chloride solution and an aluminum chloride solution, mixing the magnesium chloride solution and the aluminum chloride solution, adding carbon nanotubes and stirring evenly to prepare a mixed salt solution;
[0014] S2: dissolving sodium hydroxide in deionized water to obtain a sodium hydroxide solution, and then slowly dropping the sodium hydroxide solution into the mixed salt solution obtained in step S1 under stirring conditions, controlling the pH to 9 to 10, and stirring the reaction for 2 to 4 hours;
[0015] S3: After the reaction is completed, the reaction solution is filtered, washed, and dried to obtain a layered double hydroxide.
[0016] Furthermore, the mass ratio of the magnesium chloride, aluminum chloride and carbon nanotubes is 1.2-1.8:1:1.5-2.
[0017] Furthermore, the inorganic pigment is one or more of titanium dioxide, iron oxide, chrome yellow and carbon black.
[0018] Furthermore, the dispersant is one or more of polyethylene wax, oleamide, stearate
[0019] Furthermore, the antioxidant is one or more of antioxidant 1010, antioxidant 1035, antioxidant 1076, antioxidant 1024.
[0020] The present application also provides a method for preparing a high-toughness antioxidant flame-retardant masterbatch, which is characterized by comprising the following steps:
[0021] Step 1: Add inorganic pigment, layered double hydroxide, talcum powder, dispersant and antioxidant into a high-speed mixer, and pre-mix at a certain temperature and a high speed for a period of time to make the components fully mixed;
[0022] Step 2: Add the premixed materials in step 1 and ethylene-vinyl acetate copolymer into a segmented twin-screw extruder, heat, melt and mix, and then extrude and granulate. After the extruded strips are cooled in air, they are pelletized to obtain the high-toughness, antioxidant and flame-retardant masterbatch.
[0023] Furthermore, in the step 1, the temperature of the mixer is 50-80°C, the rotation speed is 1000-2000 rpm, and the mixing time is 10-20 minutes; in the step 2, the screw speed of the segmented twin-screw extruder is 300-400 rpm, the heating and melting temperature is 180-200°C, the heating and melting time is 0.5-1 hour, and the extrusion granulation temperature is 200-230°C.
[0024] Ethylene-vinyl acetate copolymer (EVA) has good flexibility and elasticity, and its molecular chain contains flexible ethylene segments and polar vinyl acetate segments. When subjected to force, these segments can undergo certain deformation and orientation, absorb and disperse external energy, thereby improving the toughness of the masterbatch. Layered double hydroxide has a nano-size effect and a layered structure, which can form an effective stress dispersion center in the material. When the material is subjected to external force, the layered structure can slip and deform, absorb and dissipate external energy, thereby improving the toughness of the masterbatch. EVA interacts with layered double hydroxide to form a certain physical cross-linking structure, which further enhances the toughness of the masterbatch. EVA and layered double hydroxide themselves have certain antioxidant properties, and some groups in their molecular structure can capture free radicals and prevent the further development of oxidation reactions. Layered double hydroxide will undergo endothermic decomposition reaction during combustion, absorb a large amount of heat, and reduce the temperature of the material surface; EVA can cooperate with flame retardants such as layered double hydroxide to form a synergistic flame retardant effect.
[0025] Beneficial effects:
[0026] The present invention provides a high-toughness antioxidant flame-retardant masterbatch, which can maintain good performance without breaking or becoming brittle even when the material is repeatedly bent or deformed, and can keep the plastic product in bright color for a long time, has strong antioxidant ability and good flame retardancy, thus providing a guarantee for the export and application of the product. DETAILED DESCRIPTION
[0027] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0028] Unless otherwise specified, the chemical reagents used in the present invention are all commercially available analytically pure.
[0029] Ethylene-vinyl acetate copolymer (ethylene content 8%; weight average molecular weight 2000Da) was purchased from Shanghai Xingyun International Trade Co., Ltd.; polyethylene (weight average molecular weight 2000Da) was purchased from Qingzhou Honghui Plastic Industry Co., Ltd.
[0030] Preparation of layered double hydroxide A:
[0031] S1: dissolving 12 g of magnesium chloride in 1 L of deionized water to obtain a magnesium chloride solution, dissolving 10 g of aluminum chloride in 1 L of deionized water to obtain an aluminum chloride solution, mixing the magnesium chloride solution and the aluminum chloride solution, adding 15 g of carbon nanotubes and stirring evenly to obtain a mixed salt solution;
[0032] S2: dissolving 20 g of sodium hydroxide in 1 L of deionized water to obtain a sodium hydroxide solution, then slowly dropping the sodium hydroxide solution into the mixed salt solution obtained in step S1 under stirring, controlling the pH to 10, and stirring the reaction for 4 hours;
[0033] S3: After the reaction is completed, the reaction solution is filtered, washed, and dried to obtain a layered double hydroxide.
[0034] Preparation of layered double hydroxide B:
[0035] The difference between the present preparation and the layered double hydroxide A is that 12 g of magnesium chloride in step S1 is replaced by 18 g of magnesium chloride, and 15 g of carbon nanotubes is replaced by 20 g of carbon nanotubes.
[0036] Preparation of layered double hydroxide C:
[0037] The difference between this preparation and layered double hydroxide A is that 12 g of magnesium chloride in step S1 is replaced by 8 g of magnesium chloride.
[0038] Preparation of layered double hydroxide D:
[0039] The difference between this preparation and layered double hydroxide A is that 12 g of magnesium chloride in step S1 is replaced by 20 g of magnesium chloride.
[0040] Preparation of layered double hydroxide E:
[0041] The difference between the present preparation and the layered double hydroxide A is that 15 g of carbon nanotubes in step S1 are replaced with 10 g of carbon nanotubes.
[0042] Preparation of high toughness antioxidant flame retardant masterbatch:
[0043] Step 1: Add inorganic pigment, magnesium aluminum layered double hydroxide, talcum powder, dispersant and antioxidant into a high-speed mixer, and pre-mix at 60° C. and 1500 rpm for 20 minutes to fully mix the components;
[0044] Step 2: Add the premixed materials in step 1 together with ethylene-vinyl acetate copolymer into a segmented twin-screw extruder, the screw speed of the segmented twin-screw extruder is 350 rpm, and the mixture is heated, melted and mixed before extrusion and granulation. The heating and melting temperature is 180°C, the heating and melting time is 0.5 hours, the extrusion granulation temperature is 200°C, and the extruded strips are cooled in the air and then pelletized to obtain the high-toughness antioxidant flame-retardant masterbatch.
[0045] Examples 1 to 6
[0046] According to the above-mentioned preparation method of high-toughness antioxidant flame-retardant masterbatch, Table 1 is the ingredient list of high-toughness antioxidant flame-retardant masterbatch of Examples 1 to 6 in parts by weight.
[0047] Table 1
[0048]
[0049] Comparative Example 1:
[0050] Comparative Example 1 was prepared according to the above method for preparing high-toughness antioxidant flame-retardant masterbatch. The difference between this preparation and Example 2 is that no layered double hydroxide was added.
[0051] Comparative Example 2:
[0052] Comparative Example 2 was prepared according to the above-mentioned method for preparing high-toughness antioxidant flame-retardant masterbatch. The difference between this preparation and Example 2 is that ethylene-vinyl acetate copolymer (ethylene content 8%; weight average molecular weight 2000Da) was replaced by polyethylene (weight average molecular weight 2000Da).
[0053] Performance test: The high-toughness antioxidant flame-retardant masterbatches prepared in Examples 1 to 6 and Comparative Examples 1 to 2 were tested for tensile strength, antioxidant properties, and flame retardancy. The test methods are as follows:
[0054] 1. Tensile strength test:
[0055] According to the standard (such as ISO 527), the masterbatch is prepared into a 2×5×10 cm long strip sample. The sample is stretched at a tensile speed of 1 cm per minute using a universal material testing machine until the sample breaks. The force and displacement data during the stretching process are obtained to calculate the tensile strength.
[0056] 2. Antioxidant performance test:
[0057] Use a differential scanning calorimeter (DSC) to measure the oxidation induction time of masterbatch in an oxygen atmosphere. Weigh 10 mg of masterbatch sample, put it in the DSC sample pan, set the experimental parameters, set the heating rate to 20℃ / min, start DSC, heat the sample to the set temperature of 230℃, and then introduce oxygen at an oxygen flow rate of 50mL / min. The instrument will record the change of the heat flow of the sample over time. When the sample begins to oxidize, the heat flow will change significantly. The time from the introduction of oxygen to the change in heat flow is the oxidation induction time. The longer the oxidation induction time, the better the antioxidant performance of the material.
[0058] 3. Flame retardancy test:
[0059] According to the relevant standards (UL94), prepare a sample with a size of 125mm×13mm×3mm, fix the sample vertically on the fixture of the combustion box, ensure that the lower end of the sample is a certain distance from the top of the burner, and adjust the flame height and temperature of the burner according to the standard requirements. The blue inner flame height is 20mm, the outer flame height is 40mm, and the temperature is about 550℃. Carry out a combustion test, ignite the lower end of the sample, and observe the combustion behavior of the sample. Record the burning time, burning length, dripping and other parameters of the sample. Evaluation level: According to the parameters such as burning time and burning length, the flame retardant performance of the sample is evaluated according to the standard. It is divided into V-0, V-1, and V-2 levels. V-0 level indicates the best flame retardant performance, V-1 level indicates general flame retardant performance, and V-2 level indicates the worst flame retardant performance.
[0060] Table 2: Test results
[0061]
[0062]
[0063] From the above data, it can be seen that the high-toughness antioxidant flame-retardant masterbatch of Examples 1 to 3 has good tensile strength, oxidation resistance and flame retardancy; from the comparison between Example 4 and Example 2, it can be seen that when preparing the layered double hydroxide, there is too little magnesium chloride, and the mass ratio of magnesium chloride, aluminum chloride and carbon nanotubes is unreasonable, which will make the tensile strength, oxidation resistance and flame retardancy of the prepared high-toughness antioxidant flame-retardant masterbatch worse; from the comparison between Example 5 and Example 2, it can be seen that when preparing the layered double hydroxide, there is too much magnesium chloride, and the mass ratio of magnesium chloride, aluminum chloride and carbon nanotubes is unreasonable, which will make the tensile strength, oxidation resistance and flame retardancy of the prepared high-toughness antioxidant flame-retardant masterbatch worse; from the comparison between Example 6 and Example 7, the tensile strength, oxidation resistance and flame retardancy of the prepared high-toughness antioxidant flame-retardant masterbatch worse. From Example 2, it can be seen that when preparing layered double hydroxide, there are too few carbon nanotubes, and the mass ratio of magnesium chloride, aluminum chloride and carbon nanotubes is unreasonable, the tensile strength, oxidation resistance and flame retardancy of the prepared high-toughness antioxidant flame retardant masterbatch will be deteriorated; from the comparison between Comparative Example 1 and Example 2, it can be seen that without adding layered double hydroxide, the tensile strength, oxidation resistance and flame retardancy of the prepared high-toughness antioxidant flame retardant masterbatch will be deteriorated; from the comparison between Comparative Example 2 and Example 2, it can be seen that when ethylene-vinyl acetate copolymer (ethylene: 8%) is replaced with polyethylene, the tensile strength, oxidation resistance and flame retardancy of the prepared high-toughness antioxidant flame retardant masterbatch will be deteriorated, and the expected effect will not be achieved.
[0064] The present invention can also have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.
Claims
1. A high-toughness, antioxidant, flame-retardant masterbatch, characterized in that: The raw materials for preparing the high-toughness anti-oxidation and flame-retardant masterbatch include: inorganic pigment, ethylene-vinyl acetate copolymer, layered double hydroxide, talcum powder, dispersant and antioxidant.
2. The high-toughness, antioxidant, flame-retardant masterbatch according to claim 1, characterized in that: The raw materials for preparing the high-toughness antioxidant flame-retardant masterbatch include, by weight, 15 to 25 parts of inorganic pigment, 40 to 60 parts of ethylene-vinyl acetate copolymer, 8 to 12 parts of layered double hydroxide, 1 to 3 parts of talc, 4 to 8 parts of dispersant, and 2 to 4 parts of antioxidant.
3. The high-toughness, anti-oxidation and flame-retardant masterbatch according to claim 1, characterized in that: The mass content of ethylene in the ethylene-vinyl acetate copolymer is 8-14% of the ethylene-vinyl acetate copolymer.
4. The high-toughness, antioxidant, flame-retardant masterbatch according to claim 1, characterized in that: The layered double hydroxide is formed by the reaction of magnesium chloride, aluminum chloride, carbon nanotubes and sodium hydroxide.
5. A high toughness antioxidant flame retardant masterbatch according to claim 1 or 5, characterized in that: The preparation method of the layered double hydroxide comprises the following steps: S1: dissolving magnesium chloride and aluminum chloride in a certain amount of deionized water respectively to prepare a magnesium chloride solution and an aluminum chloride solution, mixing the magnesium chloride solution and the aluminum chloride solution, adding carbon nanotubes and stirring evenly to prepare a mixed salt solution; S2: dissolving sodium hydroxide in deionized water to obtain a sodium hydroxide solution, and then slowly dropping the sodium hydroxide solution into the mixed salt solution obtained in step S1 under stirring conditions, controlling the pH to 9 to 10, and stirring the reaction for 2 to 4 hours; S3: After the reaction is completed, the reaction solution is filtered, washed, and dried to obtain a layered double hydroxide.
6. The high-toughness, anti-oxidation and flame-retardant masterbatch according to claim 5, characterized in that: The mass ratio of the magnesium chloride, aluminum chloride and carbon nanotubes is 1.2-1.8:1:1.5-2.
7. The high-toughness, anti-oxidation and flame-retardant masterbatch according to claim 1, characterized in that: The inorganic pigment is one or more of titanium dioxide, iron oxide, chrome yellow and carbon black.
8. The high-toughness, anti-oxidation and flame-retardant masterbatch according to claim 1, characterized in that: The dispersant is one or more of polyethylene wax, oleamide, and stearate; the antioxidant is one or more of antioxidant 1010, antioxidant 1035, antioxidant 1076, and antioxidant 1024.
9. The method for preparing a high-toughness, antioxidant, flame-retardant masterbatch according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1: Add inorganic pigment, layered double hydroxide, talcum powder, dispersant and antioxidant into a high-speed mixer, and pre-mix at a certain temperature and a high speed for a period of time to make the components fully mixed; Step 2: Add the premixed materials in step 1 and ethylene-vinyl acetate copolymer into a segmented twin-screw extruder, heat, melt and mix, and then extrude and granulate. After the extruded strips are cooled in air, they are pelletized to obtain the high-toughness, antioxidant and flame-retardant masterbatch.
10. The method for preparing a high-toughness, antioxidant, flame-retardant masterbatch according to claim 9, characterized in that: In the step 1, the mixer temperature is 50-80°C, the rotation speed is 1000-2000 rpm, and the mixing time is 10-20 minutes; in the step 2, the screw speed of the segmented twin-screw extruder is 300-400 rpm, the heating and melting temperature is 180-200°C, the heating and melting time is 0.5-1 hour, and the extrusion granulation temperature is 200-230°C.
Citation Information
Cited By
Flame-retardant antioxidant color master batch and preparation method thereof
CN119978458A