High-strength flame-retardant epoxy resin composition suitable for HP-RTM process and preparation method of high-strength flame-retardant epoxy resin composition

By using a composition of phosphate ester compounds and tetrabromobenzene A epoxy resin in the HP-RTM process, combined with a specific group distribution ratio, the problem of difficult to take into account both flame retardant properties and mechanical properties in the prior art is achieved. The preparation of high-strength flame retardant epoxy resin has been improved, and the overall performance of automotive materials has been improved.

CN119081357APending Publication Date: 2024-12-06四川东树新材料有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411199842.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing epoxy resin curing system suitable for HP-RTM process not only improves flame retardant performance, but also sacrifices mechanical properties, especially the bending mechanical properties, making it difficult to meet the high flame retardant and high mechanical strength at the same time. Require.

Method used

The composition of phosphate compounds and tetrabromobenzene A epoxy resin is used as the flame retardant, and is controlled by the mass ratio of specific components A and components B, and is combined with matrix resin, diluent, additive, and amine curing. The ratio of the agent and the accelerator is to prepare a high-strength flame retardant epoxy resin composition, which is suitable for the HP-RTM process.

Benefits of technology

The excellent flame retardant properties of the epoxy resin composition are achieved and the high mechanical strength are improved, including improving the tensile and bending properties of the cast body, and meeting the high-efficiency molding needs of lightweight materials in automobiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005017568480000071
    Figure BDA0005017568480000071
Patent Text Reader

Abstract

The invention discloses a high-strength flame-retardant epoxy resin composition suitable for an HP-RTM process, the high-strength flame-retardant epoxy resin composition comprises a component A and a component B. The component A comprises matrix resin, a flame retardant, a diluent and an auxiliary agent, the component B comprises an amine curing agent and an accelerant, the flame retardant is a composition of a phosphate compound and tetrabromobisphenol A epoxy resin, and the diluent is a composition of an amine curing agent and a tetrabromobisphenol A epoxy resin. The mass ratio of the phosphate ester compound to the tetrabromobisphenol A epoxy resin is (5-20): (25-40), and the component A and the component B are mixed according to the mass ratio of (4-5): 1 when the high-strength flame-retardant epoxy resin composition suitable for the HP-RTM process is used. The preparation method comprises the following steps: uniformly mixing the matrix resin, the flame retardant, the diluent and the assistant in proportion to obtain a component A; uniformly mixing an amine curing agent and an accelerant in proportion to obtain a component B; the prepared epoxy resin composition has excellent flame retardance and also has high mechanical strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of epoxy resins, and in particular relates to a high-strength flame-retardant epoxy resin composition suitable for HP-RTM process and a preparation method thereof. Background Art

[0002] As we all know, the fuel consumption of a vehicle is closely related to its own weight. Without affecting the strength and safety performance of the vehicle, reducing the weight of the vehicle as much as possible will help reduce the fuel consumption per 100 kilometers and increase the cruising range of new energy vehicles. Against the backdrop of my country's increasing emphasis on and efforts to control environmental pollution, lightweighting of vehicles has become a trend.

[0003] Up to now, the materials that can be used for lightweight design applications of automobiles mainly include high-strength steel, lightweight alloys and composite materials. Among them, the comprehensive performance of resin-based composite materials with reinforcements such as glass fiber and carbon fiber exceeds that of lightweight alloys and high-strength steel, and they are ideal lightweight materials for automobiles. However, the traditional molding process cycle of epoxy resin-based composite materials is as long as several hours, which is far from meeting the high efficiency requirements of automobile production lines. In contrast, the HP-RTM molding process (high-pressure resin transfer molding process) can produce composite materials for automobiles within 5-10 minutes, greatly shortening the production cycle.

[0004] Nowadays, epoxy resin curing systems suitable for HP-RTM process need to sacrifice some mechanical properties under the condition of improving their flame retardant properties. For example, patent CN116162326A discloses a system suitable for HP-RTM process, which can achieve rapid curing and molding while also obtaining high flame retardant properties. However, the tensile strength of the casting prepared by this method is only 59-63MPa, and no bending mechanical properties are provided. For another example, patent CN118006086A discloses an epoxy resin composition suitable for HP-RTM molding process and its preparation method and application. The epoxy resin composition can be rapidly cured within 100-150°C, is suitable for HP-RTM molding process, and the composite material made of fiber fabric has excellent flame retardant properties, resistance to wet and hot aging and mechanical properties. The system also does not publish bending mechanical data. It is urgent to develop an epoxy resin composition with both high flame retardant properties and high mechanical strength. Summary of the invention

[0005] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.

[0006] In order to achieve these purposes and other advantages according to the present invention, a high-strength flame-retardant epoxy resin composition suitable for HP-RTM process is provided, characterized in that it comprises component A and component B, wherein the component A comprises a base resin, a flame retardant, a diluent and an auxiliary agent, the component B comprises an amine curing agent and an accelerator, the flame retardant is a composition of a phosphate compound and a tetrabromobisphenol A epoxy resin, the mass ratio of the phosphate compound to the tetrabromobisphenol A epoxy resin is 5-20:25-40, and the high-strength flame-retardant epoxy resin composition suitable for HP-RTM process is mixed at a mass ratio of component A to component B of 4-5:1 when used.

[0007] Preferably, in the component A, the mass ratio of the base resin, the flame retardant, the diluent and the auxiliary agent is 30-70:30-70:5-20:0.5-2.

[0008] Preferably, in the component B, the mass ratio of the amine curing agent to the accelerator is 70-95:5-30.

[0009] Preferably, the base resin is one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, alicyclic epoxy resin, multifunctional epoxy resin, brominated epoxy resin, novolac epoxy resin and cardanol epoxy resin.

[0010] Preferably, the phosphate ester compound is triethyl phosphate and triphenyl phosphate, and the mass ratio of the triethyl phosphate to the triphenyl phosphate is 1:1.

[0011] Preferably, the diluent is one or more of a monofunctional epoxy diluent, a difunctional epoxy diluent, a multifunctional epoxy diluent, a low molecular weight polypropylene glycol, a low molecular weight polyethylene glycol, a low molecular weight multifunctional polyol and a low molecular weight ester compound.

[0012] Preferably, the auxiliary agent is one or more of 3-glycidylpropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, N-2(aminoethyl)3-aminopropyltrimethoxysilane, polysiloxane or fluorine-grafted modified siloxane.

[0013] Preferably, the amine curing agent is one or more of diethylamine, diethylenetriamine, divinylpropylamine, triethylamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, polyethylenepolyamine, diaminodiphenylmethane, meta-phenylenediamine, diaminodiphenyl sulfone, meta-phenylenediamine, dicyandiamide, 1,3-cyclohexanedimethylamine, and 4,4-diaminodicyclohexylmethane.

[0014] Preferably, the accelerator is one or more of a tertiary amine, an imidazole, a quaternary ammonium salt or a phosphonium salt.

[0015] A method for preparing the high-strength flame-retardant epoxy resin composition suitable for the HP-RTM process comprises:

[0016] S1. The base resin, flame retardant, diluent and additive are mixed uniformly in proportion, and reacted at a speed of 100 to 300 r / min and a temperature of 60 to 70° C. for 3 to 4 hours to prepare component A;

[0017] S2, the amine curing agent and the accelerator are mixed uniformly in proportion, and reacted at a speed of 100 to 300 r / min and a temperature of 30 to 70° C. for 2 to 3 hours to prepare component B;

[0018] Components A and B should be mixed when in use and stored separately.

[0019] The present invention has at least the following beneficial effects: by using a composition of a phosphate compound and tetrabromobisphenol A epoxy resin as a flame retardant and controlling the mass ratio of component A to component B, the epoxy resin composition prepared can have excellent flame retardancy and high mechanical strength.

[0020] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. DETAILED DESCRIPTION

[0021] The present invention is described in further detail below so that those skilled in the art can implement it according to the description.

[0022] Example 1

[0023] A method for preparing a high-strength flame-retardant epoxy resin composition suitable for an HP-RTM process comprises: S1, uniformly mixing 35 kg of bisphenol A epoxy resin, 10 kg of bisphenol F epoxy resin, 4 kg of triethyl phosphate, 4 kg of triphenyl phosphate, 33 kg of tetrabromobisphenol A epoxy resin (NPEB-400), 6 kg of difunctional epoxy diluent 1,4-butanediol diglycidyl ether, 7 kg of difunctional epoxy diluent 1,6-butanediol diglycidyl ether, and 1 kg of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and reacting the mixture at a speed of 200 r / min and a temperature of 70°C for 3 hours to prepare component A.

[0024] S2. Evenly mix 75 kg of polyethylene polyamine and 25 kg of 2-methyl-4-ethylimidazole, and react them at a speed of 200 r / min and a temperature of 50°C for 2 hours to prepare component B. Component A and component B are stored separately. When used, component A and component B are mixed at a mass ratio of 5:1, and then cast.

[0025] Example 2

[0026] A method for preparing a high-strength flame-retardant epoxy resin composition suitable for an HP-RTM process comprises: S1, uniformly mixing 35 kg of bisphenol A epoxy resin, 10 kg of bisphenol F epoxy resin, 6 kg of triethyl phosphate, 6 kg of triphenyl phosphate, 29 kg of tetrabromobisphenol A epoxy resin (NPEB-400), 6 kg of difunctional epoxy diluent 1,4-butanediol diglycidyl ether, 7 kg of difunctional epoxy diluent 1,6-butanediol diglycidyl ether, and 1 kg of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and reacting the mixture at a speed of 200 r / min and a temperature of 70°C for 3 hours to prepare component A.

[0027] S2. Evenly mix 75 kg of polyethylene polyamine and 25 kg of 2-methyl-4-ethylimidazole, and react them at a speed of 200 r / min and a temperature of 50°C for 2 hours to prepare component B. Component A and component B are stored separately. When used, component A and component B are mixed at a mass ratio of 5:1, and then cast.

[0028] Example 3

[0029] A method for preparing a high-strength flame-retardant epoxy resin composition suitable for an HP-RTM process comprises: S1, uniformly mixing 35 kg of bisphenol A epoxy resin, 10 kg of bisphenol F epoxy resin, 8 kg of triethyl phosphate, 8 kg of triphenyl phosphate, 25 kg of tetrabromobisphenol A epoxy resin (NPEB-400), 6 kg of difunctional epoxy diluent 1,4-butanediol diglycidyl ether, 7 kg of difunctional epoxy diluent 1,6-butanediol diglycidyl ether, and 1 kg of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and reacting the mixture at a speed of 200 r / min and a temperature of 70°C for 3 hours to prepare component A.

[0030] S2. Evenly mix 75 kg of polyethylene polyamine and 25 kg of 2-methyl-4-ethylimidazole, and react them at a speed of 200 r / min and a temperature of 50°C for 2 hours to prepare component B. Component A and component B are stored separately. When used, component A and component B are mixed at a mass ratio of 5:1, and then cast.

[0031] Comparative Example 1

[0032] A method for preparing a high-strength flame-retardant epoxy resin composition suitable for an HP-RTM process comprises: S1, uniformly mixing 44 kg of bisphenol A epoxy resin, 18 kg of bisphenol F epoxy resin, 2 kg of triethyl phosphate, 2 kg of triphenyl phosphate, 20 kg of tetrabromobisphenol A epoxy resin (NPEB-400), 6 kg of 1,4-butanediol diglycidyl ether, 7 kg of 1,6-butanediol diglycidyl ether, and 1 kg of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and reacting the mixture at a speed of 200 r / min and a temperature of 70° C. for 3 hours to prepare component A.

[0033] S2. Evenly mix 75 kg of polyethylene polyamine and 25 kg of 2-methyl-4-ethylimidazole, and react them at a speed of 200 r / min and a temperature of 50°C for 2 hours to prepare component B. Component A and component B are stored separately. When used, component A and component B are mixed at a mass ratio of 5:1, and then cast.

[0034] Comparative Example 2

[0035] A method for preparing a high-strength flame-retardant epoxy resin composition suitable for an HP-RTM process comprises: S1, uniformly mixing 15 kg of bisphenol A epoxy resin, 5 kg of bisphenol F epoxy resin, 18 kg of triethyl phosphate, 18 kg of triphenyl phosphate, 30 kg of tetrabromobisphenol A epoxy resin (NPEB-400), 6 kg of 1,4-butanediol diglycidyl ether, 7 kg of 1,6-butanediol diglycidyl ether, and 1 kg of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and reacting the mixture at a speed of 200 r / min and a temperature of 70°C for 3 hours to prepare component A.

[0036] S2. Evenly mix 75 kg of polyethylene polyamine and 25 kg of 2-methyl-4-ethylimidazole, and react them at a speed of 200 r / min and a temperature of 50°C for 2 hours to prepare component B. Component A and component B are stored separately. When used, component A and component B are mixed at a mass ratio of 5:1, and then cast.

[0037] Comparative Example 3

[0038] A method for preparing a high-strength flame-retardant epoxy resin composition suitable for an HP-RTM process comprises: S1, uniformly mixing 35 kg of bisphenol A epoxy resin, 10 kg of bisphenol F epoxy resin, 4 kg of triethyl phosphate, 4 kg of triphenyl phosphate, 33 kg of tetrabromobisphenol A epoxy resin (NPEB-400), 6 kg of 1,4-butanediol diglycidyl ether, 7 kg of 1,6-butanediol diglycidyl ether, and 1 kg of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and reacting the mixture at a speed of 200 r / min and a temperature of 70°C for 3 hours to prepare component A.

[0039] S2. Evenly mix 75 kg of polyethylene polyamine and 25 kg of 2-methyl-4-ethylimidazole, and react them at a speed of 200 r / min and a temperature of 50°C for 2 hours to prepare component B. Component A and component B are stored separately. When used, component A and component B are mixed at a mass ratio of 3:1, and then cast.

[0040] Comparative Example 4

[0041] A method for preparing a high-strength flame-retardant epoxy resin composition suitable for an HP-RTM process comprises: S1, uniformly mixing 10 kg of bisphenol A epoxy resin, 35 kg of bisphenol F epoxy resin, 0 kg of triethyl phosphate, 0 kg of triphenyl phosphate, 41 kg of tetrabromobisphenol A epoxy resin (NPEB-400), 6 kg of 1,4-butanediol diglycidyl ether, 7 kg of 1,6-butanediol diglycidyl ether, and 1 kg of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and reacting the mixture at a speed of 200 r / min and a temperature of 70°C for 3 hours to prepare component A.

[0042] S2. Evenly mix 75 kg of polyethylene polyamine and 25 kg of 2-methyl-4-ethylimidazole, and react them at a speed of 200 r / min and a temperature of 50°C for 2 hours to prepare component B. Component A and component B are stored separately. When used, component A and component B are mixed at a mass ratio of 5:1, and then cast.

[0043] Comparative Example 5

[0044] A method for preparing a high-strength flame-retardant epoxy resin composition suitable for an HP-RTM process comprises: S1, uniformly mixing 35 kg of bisphenol A epoxy resin, 10 kg of bisphenol F epoxy resin, 20.5 kg of triethyl phosphate, 20.5 kg of triphenyl phosphate, 0 kg of tetrabromobisphenol A epoxy resin (NPEB-400), 6 kg of difunctional epoxy diluent 1,4-butanediol diglycidyl ether, 7 kg of difunctional epoxy diluent 1,6-butanediol diglycidyl ether, and 1 kg of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, reacting the mixture at a speed of 200 r / min and a temperature of 70°C for 3 hours to prepare component A.

[0045] S2. Evenly mix 75 kg of polyethylene polyamine and 25 kg of 2-methyl-4-ethylimidazole, and react them at a speed of 200 r / min and a temperature of 50°C for 2 hours to prepare component B. Component A and component B are stored separately. When used, component A and component B are mixed at a mass ratio of 5:1, and then cast.

[0046] Components A and B of Examples 1 to 3 and Comparative Examples 1 to 5 were mixed and cast, and then cured at 25°C × 12h + 70°C × 2h + 120°C × 1h to prepare casting plates, which were then subjected to the following tests.

[0047] (1) Gel time: According to ASTM D 2471, the gel time tester was used to test the gel time at 110°C.

[0048] (2) Tensile properties of castings: Referring to GB / T 1040.2, the tensile strength and tensile modulus of the casting plates were tested using a universal testing machine.

[0049] (3) Bending properties of castings: Referring to GB / T 9341, the bending strength and tensile modulus of the casting plates were tested using a universal testing machine.

[0050] (4) Flame retardant performance: With reference to UL 94-2018, the flame retardancy of the casting specimens was tested using a horizontal vertical combustion instrument.

[0051] The test results are shown in Table 1:

[0052] Table 1

[0053]

[0054] Compared with Example 1, Examples 2-3 adjust the proportion of phosphate compounds and tetrabromobisphenol A epoxy resin within the range, and the flame retardancy and tensile bending mechanical properties of the prepared casting strips are both high; Compared with Example 1, Comparative Example 1 reduces the proportion of flame retardant components in the system, which will cause the flame retardancy to decrease from V0 to V1, but the tensile bending strength remains basically unchanged; Compared with Example 1, Comparative Example 2 increases the proportion of flame retardant components in the system, but reduces the content of tetrabromobisphenol A in the flame retardant components, and the tensile bending performance will decrease, but the flame retardancy remains basically unchanged and is still V0; Compared with Example 1, Comparative Example 3 changes the mass ratio of component A to component B, which will cause the tensile bending performance to decrease, but the flame retardancy decreases between V1 and V0; Compared with Example 1, Comparative Example 4 does not add phosphate flame retardant, which will cause the flame retardancy to decrease from V0 to V1, but the tensile bending strength remains basically unchanged; Compared with Example 1, Comparative Example 5 does not add tetrabromobisphenol A flame retardant, which will cause the flame retardancy to decrease from V0 to V1, and the tensile bending strength will also decrease.

[0055] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.

Claims

1. A high-strength flame-retardant epoxy resin composition suitable for HP-RTM process, characterized in that: The invention comprises component A and component B, wherein the component A comprises a base resin, a flame retardant, a diluent and an auxiliary agent, the component B comprises an amine curing agent and an accelerator, the flame retardant is a composition of a phosphate compound and a tetrabromobisphenol A epoxy resin, the mass ratio of the phosphate compound to the tetrabromobisphenol A epoxy resin is 5-20:25-40, and the high-strength flame-retardant epoxy resin composition suitable for the HP-RTM process is mixed at a mass ratio of component A to component B of 4-5:1 when used.

2. The high-strength flame-retardant epoxy resin composition suitable for HP-RTM process according to claim 1, characterized in that: In the component A, the mass ratio of the base resin, the flame retardant, the diluent and the auxiliary agent is 30-70:30-70:5-20:0.5-2.

3. The high-strength flame-retardant epoxy resin composition suitable for HP-RTM process according to claim 1, characterized in that: In the B component, the mass ratio of the amine curing agent to the accelerator is 70-95:5-30.

4. The high-strength flame-retardant epoxy resin composition suitable for HP-RTM process according to claim 1, characterized in that: The base resin is one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, alicyclic epoxy resin, multifunctional epoxy resin, brominated epoxy resin, novolac epoxy resin and cardanol epoxy resin.

5. The high-strength flame-retardant epoxy resin composition suitable for HP-RTM process according to claim 1, characterized in that: The phosphate ester compounds are triethyl phosphate and triphenyl phosphate, and the mass ratio of the triethyl phosphate to the triphenyl phosphate is 1:

1.

6. The high-strength flame-retardant epoxy resin composition suitable for HP-RTM process according to claim 1, characterized in that: The diluent is one or more of a monofunctional epoxy diluent, a difunctional epoxy diluent, a multifunctional epoxy diluent, a low molecular weight polypropylene glycol, a low molecular weight polyethylene glycol, a low molecular weight multifunctional polyol and a low molecular weight ester compound.

7. The high-strength flame-retardant epoxy resin composition suitable for HP-RTM process according to claim 1, characterized in that: The auxiliary agent is one or more of 3-glycidylpropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, N-2(aminoethyl)3-aminopropyltrimethoxysilane, polysiloxane or fluorine-grafted modified siloxane.

8. The high-strength flame-retardant epoxy resin composition suitable for HP-RTM process according to claim 1, characterized in that: The amine curing agent is one or more of diethylamine, diethylenetriamine, divinylpropylamine, triethylamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, polyethylenepolyamine, diaminodiphenylmethane, meta-phenylenediamine, diaminodiphenyl sulfone, meta-phenylenediamine, dicyandiamide, 1,3-cyclohexanedimethylamine, and 4,4-diaminodicyclohexylmethane.

9. The high-strength flame-retardant epoxy resin composition suitable for HP-RTM process according to claim 1, characterized in that: The accelerator is one or more of tertiary amine, imidazole, quaternary ammonium salt or phosphonium salt.

10. A method for preparing a high-strength flame-retardant epoxy resin composition suitable for HP-RTM process according to any one of claims 1 to 9, comprising: S1. The base resin, flame retardant, diluent and additive are mixed uniformly in proportion, and reacted at a speed of 100 to 300 r / min and a temperature of 60 to 70° C. for 3 to 4 hours to prepare component A; S2, the amine curing agent and the accelerator are mixed uniformly in proportion, and reacted at a speed of 100 to 300 r / min and a temperature of 30 to 70° C. for 2 to 3 hours to prepare component B; Components A and B should be mixed when in use and stored separately.

Citation Information

Cited By

  • Flame-retardant fast-curing epoxy resin composition, preparation method thereof and composite material based on epoxy resin composition

    CN121006031A