Antistatic, halogen-free, flame-retardant and heat-resistant PC / ABS alloy material and preparation method thereof

Through the combination of halogen-free flame-retardant smoke density inhibitor and antistatic agent, the shortcomings of PC/ABS alloy materials in flame retardant and heat resistance are solved, and efficient halogen-free flame retardant and antistatic properties are achieved, which is suitable for Various industrial applications.

CN119081382APending Publication Date: 2024-12-06QINGDAO GON TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411208149.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing PC/ABS alloy materials have shortcomings in flame retardant properties and heat resistance, especially in applications in electronic and electrical fields. Traditional halogen smoke density inhibitors will produce toxic gases and produce large smoke, which will affect safety. and processing performance.

Method used

Using a combination of halogen-free flame retardant smoke density inhibitors, including nano-scale powdered materials such as magnesium carbonate, ammonium manganate and alkaline aluminum oxalate, dilute oxygen by diluting gas and water vapor, forming a protective layer to prevent oxygen and heat The melt blending and extrusion process is carried out in combination with specific process conditions.

Benefits of technology

It realizes good flame retardant effects of anti-static, halogen-free flame retardant and heat-resistant PC/ABS alloy materials (UL94 fire resistance level reaches V-0), while maintaining good mechanical properties, weather resistance and anti-static properties, suitable for Thin-walled products and large parts fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of PC / ABS alloy materials, and particularly relates to an antistatic, halogen-free, flame-retardant and heat-resistant PC / ABS alloy material and a preparation method thereof. The antistatic, halogen-free, flame-retardant and heat-resistant PC / ABS alloy material comprises the following raw materials in parts by weight: 60-80 parts of PC; 20 to 40 parts of ABS (acrylonitrile butadiene styrene); 10 to 25 parts of a smoke density inhibitor; 2-5 parts of a heat-resistant agent; 1-3 parts of an antistatic agent; 2-8 parts of a compatibilizer; 3-1 part of a coupling agent; 0.3 to 1 part of a lubricant; and 0.3 to 1 part of an antioxidant. The antistatic, halogen-free, flame-retardant and heat-resistant PC / ABS alloy material provided by the invention has a good flame-retardant effect (UL94 fireproof grade reaches V-0), and good mechanical properties, weather resistance, antistatic performance and heat resistance are ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of PC / ABS alloy materials, and specifically relates to an antistatic, halogen-free, flame-retardant and heat-resistant PC / ABS alloy material and a preparation method thereof. Background Art

[0002] Polycarbonate (PC) is a thermoplastic engineering plastic with excellent comprehensive properties. It has the characteristics of high temperature resistance, flame retardancy, good electrical insulation, dimensional stability, non-toxicity and odorlessness. However, PC also has disadvantages such as high melt viscosity, poor fluidity, notch sensitivity, easy stress cracking, poor resistance to organic chemicals, and high price, which limit its application in many fields.

[0003] ABS combines the performance of three monomers. It has good low-temperature impact resistance, chemical resistance and molding processing performance, and is relatively cheap. It is widely used in automobiles, electrical appliances, instruments and other fields. However, it has disadvantages such as poor flame retardancy, high temperature resistance and weather resistance.

[0004] PC / ABS alloy is the earliest polycarbonate modified product to achieve industrial production and is an important engineering plastic alloy. PC / ABS alloy combines the advantages of PC and ABS. On the one hand, the alloy can improve the heat resistance and tensile strength of ABS. On the other hand, it can also reduce the melt viscosity of PC and improve the processing performance. It can be used to form large-area and complex products. At the same time, it can reduce the internal stress of the products and improve the low-temperature impact resistance. PC / ABS alloy materials have been widely used in the automotive industry and are the most suitable interior materials for automobiles, especially as raw materials for dashboard brackets, covers, vents, brackets, radiator grilles, and steering column protective covers. At present, PC / ABS is also widely used in industries such as computers, communication tools, and office equipment.

[0005] The flame retardancy of PC / ABS alloys has been a hot topic in the development of PC / ABS in recent years. PC itself has certain flame retardancy (limiting oxygen index LOI = 25), but after blending with ABS (limiting oxygen index LOI = 18.5), the flame retardancy decreases. In order to meet the application of PC / ABS alloys in electronics, electrical switches, electrical appliances and other fields, smoke density inhibitors must be added. Common flame retardant PC / ABS materials include synergistic systems composed of halogen smoke density inhibitors (such as tetrabromobisphenol A, brominated epoxy oligomers, decabromodiphenyl ether, decabromodiphenylethane, etc.) and antimony oxide. PC / ABS is given high flame retardancy, but it has a large amount of smoke and produces toxic and corrosive gases, which hinder rescue and personnel evacuation, leading to secondary disasters. At present, there are many reports on halogen-free flame retardant PC / ABS alloy materials using phosphorus smoke density inhibitors, nitrogen-phosphorus smoke density inhibitors, and silicon-based smoke density inhibitors. However, due to the high addition amount, the various mechanical properties and processing fluidity of the material are seriously deteriorated, resulting in a narrower processing window. The application of such products in some thin-walled products and large parts is limited to a certain extent.

[0006] In addition, the high insulation and easy accumulation of static electricity (surface resistivity is 4×1020Ω) of PC / ABS itself greatly limit its application. Some parts of electronic and electrical products, lighting equipment, automobiles, etc. have high requirements for heat resistance.

[0007] Therefore, developing an antistatic, halogen-free, flame-retardant, and heat-resistant PC / ABS has become the future development direction. Summary of the invention

[0008] In view of the above technical problems, the present invention provides an antistatic, halogen-free flame-retardant, heat-resistant PC / ABS alloy material and a preparation method thereof. The antistatic, halogen-free flame-retardant, heat-resistant PC / ABS alloy material has good flame retardant effect (UL94 fire rating reaches V-0), and ensures good mechanical properties, weather resistance, antistatic properties and heat resistance.

[0009] The present invention is achieved through the following technical solutions:

[0010] An antistatic, halogen-free flame-retardant, heat-resistant PC / ABS alloy material, wherein the raw materials of the antistatic, halogen-free flame-retardant, heat-resistant PC / ABS alloy material include, by weight:

[0011] PC: 60-80 copies;

[0012] ABS: 20-40 parts;

[0013] Smoke density suppressant: 10-25 parts;

[0014] Heat-resistant agent: 2-5 parts;

[0015] Antistatic agent: 1-3 parts;

[0016] Compatibilizer: 2-8 parts;

[0017] Coupling agent: 0.3-1 part;

[0018] Lubricant: 0.3-1 part;

[0019] Antioxidant: 0.3-1 part.

[0020] Furthermore, in the ABS, the weight percentage of acrylonitrile is 10-30%, the weight percentage of butadiene is 10-30%, and the weight percentage of styrene is 45-65%. Specifically, the PC is polycarbonate; and the ABS is a mixture of a graft copolymer containing butadiene and acrylonitrile and styrene.

[0021] Further, the smoke density inhibitor is a mixture of magnesium carbonate and one of ammonium nonammonium manganese molybdate, basic aluminum oxalate, and capsule red phosphorus;

[0022] The magnesium carbonate, ammonium manganese nonamolybdate and alkaline aluminum oxalate in the smoke density suppressant are all in nanometer powder form, and the purity of the magnesium carbonate, ammonium manganese nonamolybdate and alkaline aluminum oxalate is greater than or equal to 99.9%. Preferably, the average particle size of the encapsulated red phosphorus used is less than 20 μm;

[0023] The smoke density inhibitor of the present invention contains magnesium carbonate and other inhibitors. The principle of flame retardancy and smoke suppression is as follows: magnesium carbonate decomposes at high temperature to release carbon dioxide and water. The released carbon dioxide gas and water vapor dilute the concentration of surrounding oxygen, so that a protective layer is formed on the surface of the object, thereby preventing further diffusion of oxygen and heat; magnesium carbonate is selected as a flame retardant, which is friendly to the human environment and does not produce toxic and harmful substances.

[0024] The magnesium carbonate, ammonium nonammonium manganate and alkaline aluminum oxalate in the smoke density inhibitor are all in nanometer-scale powder form, which increases the surface area of ​​the particles and can increase the water vapor pressure on the surface of the particles, which is beneficial to improving the flame retardancy. At the same time, the ultrafine inorganic rigid particles can enhance the interaction between the polymer and the inorganic interface, can be more evenly dispersed in the matrix resin, and have a toughening and strengthening effect on the polymer material; and the use of high-purity components can ensure the content of effective ingredients in the smoke density inhibitor, reducing the amount of smoke density inhibitor used in the alloy material.

[0025] In the present invention, the smoke density suppressant adopts any one of the first smoke density suppressant, the second smoke density suppressant and the third smoke density suppressant; in the first smoke density suppressant, the mass ratio of magnesium carbonate to ammonium nonamolybdate manganate is 1:(0.5-2); in the second smoke density suppressant, the mass ratio of magnesium carbonate to alkaline aluminum oxalate is 1:(0.5-2); in the third smoke density suppressant, the mass ratio of magnesium carbonate to capsule red phosphorus is 1:(0.5-2); preferably, in the first smoke density suppressant, the mass ratio of magnesium carbonate to ammonium nonamolybdate manganate is 1:1; in the second smoke density suppressant, the mass ratio of magnesium carbonate to alkaline aluminum oxalate is 1:1; in the third smoke density suppressant, the mass ratio of magnesium carbonate to capsule red phosphorus is 1:1.

[0026] The smoke density inhibitor provided in the present invention is an environmentally friendly halogen-free inorganic mineral smoke density inhibitor, which reduces the temperature of the material surface by absorbing heat, thereby reducing the combustion of the material, forming a carbonized layer to block heat transfer and prevent contact with oxygen; it also has flame retardant and smoke suppression effects. The smoke density inhibitor selected in the present invention is mixed with magnesium carbonate and one of ammonium nonammonium manganate, alkaline aluminum oxalate, and capsule red phosphorus. The obtained smoke density inhibitor will not affect the mechanical properties and processing fluidity of the material, and will not limit the application of the product in the field of thin-walled products and large parts.

[0027] Furthermore, the heat-resistant agent is one or both of α-methylstyrene and styrene-N-phenylmaleimide copolymer (MS-NIP).

[0028] In the present invention, the heat-resistant agent a is α-methylstyrene; the heat-resistant agent b is styrene-N-phenylmaleimide copolymer (MS-NIP); the heat-resistant agent c is α-methylstyrene and styrene-N-phenylmaleimide copolymer (MS-NIP), and the mass ratio of α-methylstyrene to styrene-N-phenylmaleimide copolymer (MS-NIP) is 1:1.

[0029] Furthermore, the antistatic agent is one or more of carbon nanotubes, alkyl sulfates, and alkyl phosphates. In the present invention, antistatic agent a is carbon nanotubes; antistatic agent b is carbon nanotubes and alkyl sulfates, with a mass ratio of 1:1; antistatic agent c is carbon nanotubes and alkyl phosphates, with a mass ratio of 1:1.

[0030] Furthermore, the compatibilizer is one or two of maleic anhydride grafted ABS and glycidyl methacrylate grafted linear low-density polyethylene (LLDPE-g-GMA).

[0031] Furthermore, the coupling agent is a titanate coupling agent, and the coupling agent includes one or both of isopropyl tri(dodecylbenzenesulfonyl) titanate and isopropyl tri(dioctyl phosphate) titanate.

[0032] Furthermore, the lubricant includes one or more of microcrystalline wax, PTFE (polytetrafluoroethylene), PETS (pentaerythritol stearate), ethylene bisstearamide, calcium stearate, and zinc stearate.

[0033] Furthermore, the antioxidant is one or more of 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and tris[2,4-di-tert-butylphenyl]phosphite.

[0034] A method for preparing an antistatic, halogen-free, flame-retardant, heat-resistant PC / ABS alloy material, the method comprising:

[0035] The PC, ABS, smoke density inhibitor, heat resistant agent, antistatic agent, compatibilizer, coupling agent, lubricant and antioxidant are weighed according to the proportion and mixed evenly in a high-speed mixer, and then the mixed materials are added into a twin-screw extruder, and melt blended, extruded, water-cooled, air-cooled, dried, granulated and homogenized to obtain the antistatic, halogen-free flame-retardant and heat-resistant PC / ABS alloy material;

[0036] Among them, a blending and dispersing screw combination is selected to achieve the best dispersion effect of the alloy and the smoke density suppressant. The temperatures of each temperature zone of the extruder are: first section: 200-220°C; second section: 240-260°C; third section: 240-260°C; fourth section: 230-250°C; fifth section: 230-250°C; sixth section: 230-250°C; seventh section: 225-245°C; eighth section: 225-245°C, ninth section: 225-245°C, tenth section: 225-245°C, eleventh section: 230-240°C, die head: 240-260°C, screw aspect ratio of 35-40, screw speed of 350-500r / min

[0037] Beneficial technical effects of the present invention:

[0038] The antistatic, halogen-free flame-retardant, heat-resistant PC / ABS alloy material provided by the present invention has good flame-retardant effect (UL94 fire rating reaches V-0) and ensures good mechanical properties, weather resistance, antistatic properties and heat resistance. The surface resistivity of the prepared alloy material reaches 10 10 Ω, stable in nature, and good in long-term antistatic performance.

[0039] The antistatic, halogen-free flame-retardant and heat-resistant PC / ABS alloy material of the present invention has antistatic, low cost, high mechanical properties, stable flame retardancy and thermal stability, and has a simple production process and can be widely used in industrial production. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0041] On the contrary, the present invention covers any substitution, modification, equivalent method and scheme made on the essence and scope of the present invention as defined by the claims. Further, in order to make the public have a better understanding of the present invention, some specific details are described in detail in the detailed description of the present invention below. Those skilled in the art can fully understand the present invention without the description of these details.

[0042] The antistatic, halogen-free flame-retardant and heat-resistant PC / ABS alloy material prepared by the present invention improves the shortcomings of PC / ABS insulation, easy accumulation of static electricity, flammability, poor environmental performance and poor mechanical properties caused by the addition of smoke density inhibitor, making it more suitable for application in the fields of home appliances, decorative materials, machinery and electronics.

[0043] Example 1

[0044] Weigh 75 kg of PC and 25 kg of ABS and mix them in a high-speed mixer for 20 minutes. Add the mixed materials from the hopper to a twin-screw extruder, and then go through melt blending, extrusion, water cooling, air cooling, granulation, and homogenization.

[0045] Among them, the temperatures of each temperature zone of the extruder are: section one: 200-220°C; section two: 240-260°C; section three: 240-260°C; section four: 230-250°C; section five: 230-250°C; section six: 230-250°C; section seven: 225-245°C; section eight: 225-245°C, section nine: 225-245°C, section ten: 225-245°C, section eleven: 230-240°C, die head: 240-260°C, screw aspect ratio is 35-40, screw speed is 350-500r / min.

[0046] Example 2

[0047] Weigh PC 75KG, ABS 25KG, first smoke density inhibitor (magnesium carbonate and ammonium nonamolybdate mass ratio 1: (2-3)): 12KG, antistatic agent a (carbon nanotube): 1KG, heat resistant agent a: 2KG (α-methylstyrene;), glycidyl methacrylate grafted linear low-density polyethylene: 5KG, isopropyl tri(dioctyl phosphate) titanate: 0.5KG, pentaerythritol stearate: 0.5KG, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl alcohol ester: 0.5KG, and mix them in a high-speed mixer for 20 minutes. The mixed materials are added to the twin-screw extruder from the hopper, and are melt-blended, extruded, water-cooled, air-cooled, granulated, and homogenized.

[0048] Wherein, the process conditions are the same as in Example 1.

[0049] Example 3

[0050] Weigh PC 75KG, ABS 25KG, second smoke density inhibitor (magnesium carbonate and alkaline aluminum oxalate 1: (2-3)): 12KG, antistatic agent a (carbon nanotube): 1KG, heat resistant agent a (α-methylstyrene): 2KG, methacrylate glycidyl grafted linear low-density polyethylene: 5KG, isopropyl tri (dioctyl phosphate) titanate: 0.5KG, pentaerythritol stearate: 0.5KG, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl alcohol ester: 0.5KG, and mix them in a high-speed mixer for 20 minutes. The mixed materials are added to the twin-screw extruder from the hopper, and are melt-blended, extruded, water-cooled, air-cooled, granulated, and homogenized.

[0051] Wherein, the process conditions are the same as in Example 1.

[0052] Example 4

[0053] Weigh PC 75KG, ABS 25KG, third smoke density suppressant: 12KG (magnesium carbonate and capsule red phosphorus mass ratio is 1: (2-3)), antistatic agent a (carbon nanotube): 1KG, heat resistant agent a (α-methylstyrene): 2KG, methacrylate glycidyl grafted linear low-density polyethylene: 5KG, isopropyl tri (dioctyl phosphate) titanate: 0.5KG, pentaerythritol stearate: 0.5KG, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl alcohol ester: 0.5KG, and mix them in a high-speed mixer for 20 minutes. The mixed materials are added to the twin-screw extruder from the hopper, and are melt-blended, extruded, water-cooled, air-cooled, granulated, and homogenized.

[0054] Wherein, the process conditions are the same as in Example 1.

[0055] Example 5

[0056] Weigh PC 75KG, ABS 25KG, third smoke density suppressant: 12KG (magnesium carbonate and capsule red phosphorus mass ratio is 1: (2-3)), antistatic agent b (carbon nanotubes and alkyl sulfate, mass ratio is 1: 1): 1KG, heat resistant agent a (α-methylstyrene): 2KG, methacrylate glycidyl grafted linear low-density polyethylene: 5KG, isopropyl tri (dioctyl phosphate) titanate: 0.5KG, pentaerythritol stearate: 0.5KG, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl alcohol ester: 0.5KG, and mix them in a high-speed mixer for 20 minutes. The mixed materials are added to the twin-screw extruder from the hopper, and are melt-blended, extruded, water-cooled, air-cooled, granulated, and homogenized.

[0057] Wherein, the process conditions are the same as in Example 1.

[0058] Example 6

[0059] Weigh PC 75KG, ABS 25KG, third smoke density suppressant: 12KG (magnesium carbonate and capsule red phosphorus mass ratio is 1: (2-3)), antistatic agent c (carbon nanotubes and alkyl phosphate, mass ratio is 1: 1): 1KG, heat resistant agent a (α-methylstyrene): 2KG, methacrylate glycidyl grafted linear low-density polyethylene: 5KG, isopropyl tri (dioctyl phosphate) titanate: 0.5KG, pentaerythritol stearate: 0.5KG, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl alcohol ester: 0.5KG, and mix them in a high-speed mixer for 20 minutes. The mixed materials are added to the twin-screw extruder from the hopper, and are melt-blended, extruded, water-cooled, air-cooled, granulated, and homogenized.

[0060] Wherein, the process conditions are the same as in Example 1.

[0061] Example 7

[0062] Weigh PC 75KG, ABS 25KG, third smoke density inhibitor (magnesium carbonate and capsule red phosphorus mass ratio is 1: (2-3)): 12KG, antistatic agent c: 1KG, heat resistant agent b (styrene-N-phenylmaleimide copolymer (MS-NIP)): 4KG, methacrylate glycidyl grafted linear low-density polyethylene: 5KG, isopropyl tri (dioctyl phosphate) titanate: 0.5KG, pentaerythritol stearate: 0.5KG, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl alcohol ester: 0.5KG, and mix them in a high-speed mixer for 20 minutes. The mixed materials are added to the twin-screw extruder from the hopper, and are melt-blended, extruded, water-cooled, air-cooled, granulated, and homogenized.

[0063] Wherein, the process conditions are the same as in Example 1.

[0064] Example 8

[0065] Weigh PC75KG, ABS25KG, the third smoke density inhibitor (the mass ratio of magnesium carbonate and capsule red phosphorus is 1: (2-3)): 12KG, antistatic agent c: 1KG, heat resistant agent c (α-methylstyrene and styrene-N-phenylmaleimide copolymer (MS-NIP), α-methylstyrene and styrene-N-phenylmaleimide copolymer (MS-NIP) The mass ratio is 1:1): 5KG, methacrylate glycidyl grafted linear low-density polyethylene: 5KG, isopropyl tri (dioctyl phosphate) titanate: 0.5KG, pentaerythritol stearate: 0.5KG, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate n-octadecyl alcohol ester: 0.5KG, and mix them in a high-speed mixer for 20 minutes. The mixed materials are added to the twin-screw extruder from the hopper, and are melt-blended, extruded, water-cooled, air-cooled, granulated, and homogenized.

[0066] Wherein, the process conditions are the same as in Example 1.

[0067] The PC / ABS samples of Examples 1 to 8 were injection molded into standard specimens to test their mechanical properties; the flame retardant properties were tested according to Examples 1 to 4; the antistatic properties were compared according to Examples 1, 4, 5, and 6; and the heat resistance was compared according to Examples 1, 6, 7, and 8. See Table 1.

[0068] Table 1: Performance test results of Examples 1-8.

[0069]

[0070] From the data of Examples 1-4 in Table 1, it can be seen that the first to third smoke density inhibitors provided by the present invention all have fireproof effects, especially when the third smoke density inhibitor (magnesium carbonate and capsule red phosphorus) is used, the fireproof grade can reach V-0; from the data of Examples 1, 4-6, it can be seen that the three antistatic agents added in the present invention all have antistatic effects, among which the antistatic agent c (carbon nanotubes and alkyl phosphate) has the best antistatic effect, and the surface resistivity can reach 10-2 days. 10 Ω; and according to the data of Examples 1, 6-8, it can be seen that the three heat-resistant agents added in the present invention all have the effect of resisting thermal deformation, and the third heat-resistant agent c (using α-methylstyrene and styrene-N-phenylmaleimide copolymer (MS-NIP)) has the best heat-resistant effect.

[0071] The antistatic, halogen-free flame-retardant, heat-resistant PC / ABS alloy material prepared in Example 8 of the present invention has the best fireproof grade, antistatic and heat deformation resistance effects.

[0072] It is a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An antistatic, halogen-free, flame-retardant, heat-resistant PC / ABS alloy material, characterized in that: The raw materials of the antistatic, halogen-free flame-retardant and heat-resistant PC / ABS alloy material include, by weight: PC: 60-80 copies; ABS: 20-40 parts; Smoke density suppressant: 10-25 parts; Heat-resistant agent: 2-5 parts; Antistatic agent: 1-3 parts; Compatibilizer: 2-8 parts; Coupling agent: 0.3-1 part; Lubricant: 0.3-1 part; Antioxidant: 0.3-1 part.

2. The antistatic, halogen-free, flame-retardant, heat-resistant PC / ABS alloy material according to claim 1, characterized in that: In the ABS, the weight percentage of acrylonitrile is 10-30%, the weight percentage of butadiene is 10-30%, and the weight percentage of styrene is 45-65%.

3. The antistatic, halogen-free, flame-retardant, heat-resistant PC / ABS alloy material according to claim 1, characterized in that: The smoke density suppressant is a mixture of magnesium carbonate and one of ammonium nonamolybdate manganese, basic aluminum oxalate, and capsule red phosphorus; The magnesium carbonate, ammonium nonammonium manganese oxide and alkaline aluminum oxalate in the smoke density suppressant are all in nanometer powder form.

4. The antistatic, halogen-free, flame-retardant, heat-resistant PC / ABS alloy material according to claim 1, characterized in that: The heat-resistant agent is one or both of α-methylstyrene and styrene-N-phenylmaleimide copolymer (MS-NIP).

5. The antistatic, halogen-free, flame-retardant, heat-resistant PC / ABS alloy material according to claim 1, characterized in that: The antistatic agent is one or more of carbon nanotubes, alkyl sulfate and alkyl phosphate.

6. The antistatic, halogen-free, flame-retardant, heat-resistant PC / ABS alloy material according to claim 1, characterized in that: The compatibilizer is one or two of maleic anhydride grafted ABS and glycidyl methacrylate grafted linear low-density polyethylene (LLDPE-g-GMA).

7. The antistatic, halogen-free, flame-retardant, heat-resistant PC / ABS alloy material according to claim 1, characterized in that: The coupling agent is a titanate coupling agent, and the coupling agent includes one or two of isopropyl tri(dodecylbenzenesulfonyl) titanate and isopropyl tri(dioctyl phosphate) titanate.

8. The antistatic, halogen-free, flame-retardant, heat-resistant PC / ABS alloy material according to claim 1, characterized in that: The lubricant comprises one or more of microcrystalline wax, PTFE (polytetrafluoroethylene), PETS (pentaerythritol stearate), ethylene bis stearamide, calcium stearate and zinc stearate.

9. The antistatic, halogen-free, flame-retardant, heat-resistant PC / ABS alloy material according to claim 1, characterized in that: The antioxidant is one or more of 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and tris[2,4-di-tert-butylphenyl]phosphite.

10. A method for preparing an antistatic, halogen-free flame-retardant, heat-resistant PC / ABS alloy material, used for preparing the antistatic, halogen-free flame-retardant, heat-resistant PC / ABS alloy material according to any one of claims 1 to 9, characterized in that: The method comprises: The PC, ABS, smoke density inhibitor, heat resistant agent, antistatic agent, compatibilizer, coupling agent, lubricant and antioxidant are weighed according to the proportion and mixed evenly in a high-speed mixer, and then the mixed materials are added into a twin-screw extruder, and melt blended, extruded, water-cooled, air-cooled, dried, granulated and homogenized to obtain the antistatic, halogen-free flame-retardant and heat-resistant PC / ABS alloy material; Among them, a blending and dispersing screw combination is selected to achieve the best dispersion effect of the alloy and the smoke density suppressant. The temperatures of each temperature zone of the extruder are: section one: 200-220°C; section two: 240-260°C; section three: 240-260°C; section four: 230-250°C; section five: 230-250°C; section six: 230-250°C; section seven: 225-245°C; section eight: 225-245°C, section nine: 225-245°C, section ten: 225-245°C, section eleven: 230-240°C, die head: 240-260°C, screw aspect ratio of 35-40, screw speed of 350-500r / min.

Citation Information

Cited By

  • Needle flame flame-retardant polycarbonate composite material as well as preparation method and application thereof

    CN120795591A