Environment-friendly degradable PC / PLA alloy composition as well as preparation method and application thereof
By adding compatibility agents, toughening agents and hydrolysis inhibitors to PC/PLA alloy materials, their compatibility is improved and the melt extrusion process is solved, and the problem of poor compatibility of PC/PLA alloy materials is achieved, and high toughness is achieved and the improvement of impact resistance has expanded its application areas.
Patent Information
- Application Number
- CN202411407737.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-12-06
AI Technical Summary
The poor compatibility of existing PC/PLA alloy materials leads to insufficient impact toughness and heat resistance, which limits the application field of polylactic acid materials.
The compatibility of PC/PLA is improved by adding specific compatibility agents, toughening agents and hydrolysis inhibitors to the PC/PLA alloy material, and a high-toughness modified PC/PLA alloy is obtained through the melt extrusion process. Material.
It significantly improves the impact resistance and toughness of PC/PLA alloy materials, forms environmentally friendly and degradable materials with excellent impact resistance, and expands its application in food, drug packaging, textiles, medical and other fields.
Smart Images

Figure BDA0005077135550000021 
Figure BDA0005077135550000071 
Figure BDA0005077135550000072
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of engineering plastics, and in particular to an environmentally friendly and degradable PC / PLA alloy composition, a preparation method and application thereof. Background Art
[0002] Polylactic acid (PLA) is a biodegradable green plastic, which is mainly obtained by lactide ring opening or direct polycondensation. Due to its abundant source and compliance with green emission reduction targets, it is a recognized environmentally friendly material. It has been developed more and more rapidly in the field of engineering plastics and is widely used in food and drug packaging, textiles, medical and other industries. However, with the continuous improvement of technology, defects such as poor impact toughness, poor heat resistance and flammability of PLA have also been exposed, which have limited its application to a certain extent. Polycarbonate (PC) has good toughness and heat resistance. Blending PLA with PC can produce an alloy material with good comprehensive performance. However, since PLA is a semi-crystalline polymer and PC is an amorphous polymer, how to improve the compatibility of PC / PLA is an urgent problem to be solved.
[0003] Patent CN201010151864A discloses a halogen-free flame-retardant PC / ABS / PLA alloy, which has better strength and rigidity than ordinary flame-retardant PC / ABS, flame retardant V0, but low notch impact. Patent CN109206874A discloses a method for preparing a high-toughness flame-retardant PLA / PC alloy material, which includes PLA, PC, flame retardant, nucleation promoter, toughening agent, chain extender, transesterification promoter and processing aid, and improves the toughness of the PLA / PC alloy material by adding transesterification promoter and toughening agent, but its notch impact performance is still not high. Patent CN111087789A discloses a high-impact polycarbonate / polylactic acid resin composition and a preparation method thereof, which improves the flexibility and deformability of the substrate phase by compounding two compatibilizers, supplemented by a certain transesterification catalyst, and a specific toughening agent, and the prepared polycarbonate / polylactic acid resin composition has chemical resistance and impact performance, but its components are complex and the economic cost is high.
[0004] In summary, in order to expand the application field of polylactic acid materials, it is of great significance to provide an environmentally friendly and degradable PC / PLA alloy material with excellent impact resistance. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides an environmentally friendly and degradable PC / PLA alloy composition, a preparation method and application thereof, by adding a specific compatibilizer to the environmentally friendly and degradable alloy composition, compounding it with a toughening agent and a hydrolysis inhibitor, promoting the modified crystallization of PC / PLA, and obtaining a high-toughness modified PC / PLA alloy material with good impact resistance through melt extrusion.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides an environmentally friendly and degradable PC / PLA alloy composition, wherein the raw materials for preparing the environmentally friendly and degradable PC / PLA alloy composition include the following components in weight percentage:
[0008]
[0009] In the present invention, by adding a specific content of a compatibilizer, a toughening agent and a hydrolysis inhibitor to a composite material of PC and PLA, the compatibility of PC / PLA can be effectively improved, thereby obtaining a high-toughness PC / PLA alloy composition, and then obtaining an environmentally friendly and degradable PC / PLA alloy material with strong impact resistance. Among them, by directly compounding a specific content of a compatibilizer, a toughening agent and a hydrolysis inhibitor, a synergistic effect can be exerted, thereby significantly improving the impact resistance of the obtained PC / PLA alloy composition.
[0010] In the raw materials for preparing the environmentally friendly and degradable PC / PLA alloy composition of the present invention, the PC content is 55-85wt%, for example, it can be 55%, 58%, 60%, 62%, 65%, 70%, 75%, 78%, 80% or 83%, etc.; the PLA content is 10-40wt%, for example, it can be 12%, 15%, 18%, 20%, 25%, 30%, 32%, 35%, 38% or 40%, etc.; the compatibilizer content is 2-6wt%. %, for example, it can be 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5% or 6%; the toughening agent content is 2-10wt%, for example, it can be 2%, 3%, 3.5%, 4%, 4.5%, 5%, 6%, 7%, 8%, 9% or 10%; the hydrolysis inhibitor content is 1-3wt%, for example, it can be 1%, 1.2%, 1.5%, 1.8%, 2%, 2.2%, 2.5%, 2.8% or 3% etc.
[0011] Preferably, the PC comprises aromatic polycarbonate.
[0012] Preferably, the aromatic polycarbonate comprises at least 70% aromatic moieties.
[0013] Preferably, the PC comprises bisphenol A polycarbonate.
[0014] Preferably, the weight average molecular weight of the PC is 15000-40000, for example, 18000, 20000, 22000, 25000, 28000, 30000, 32000, 35000, 38000 or 40000.
[0015] PC is more preferably any one of Makrolon 2405, Makrolon 2407 or Makrolon 3100 from Bayer, Germany, or a combination of at least two thereof.
[0016] Preferably, the PLA includes any one of L-polylactic acid, D-polylactic acid, epoxy-modified polylactic acid or maleic anhydride-modified polylactic acid, or a combination of at least two thereof.
[0017] Preferably, the weight average molecular weight of the PLA is 15000-25000, for example, 16000, 17000, 18000, 19000, 20000, 21000, 22000, 23000 or 24000.
[0018] Preferably, the compatibilizer is an epoxy compatibilizer.
[0019] Preferably, the compatibilizer is styrene-acrylonitrile-glycidyl methacrylate.
[0020] In the present invention, the epoxy compatibilizer can effectively improve the compatibility and dispersibility of PC / PLA, and the epoxy active group can react with PC and PLA to improve the mixing uniformity and compatibility of the obtained PC / PLA alloy composition, and further improve the overall toughness of the material, thereby obtaining a PC / PLA alloy composition with excellent impact resistance.
[0021] Preferably, the toughening agent is a core-shell toughening agent.
[0022] Preferably, the core-shell toughening agent includes any one of C-223A, AX8900, S2100, BTA731, ACR, and MBS, or a combination of at least two thereof.
[0023] The addition of the specific core-shell toughening agent in the present invention can promote the modified crystallization of PC / PLA, so that a high-toughness modified PC / PLA alloy composition can be obtained after melt extrusion.
[0024] Preferably, the hydrolysis inhibitor comprises a diimine-type hydrolysis inhibitor and / or an epoxy compound hydrolysis stabilizer.
[0025] Preferably, the diimide type hydrolysis inhibitor comprises monocarbodiimide and / or polycarbodiimide.
[0026] Preferably, the epoxy compound hydrolysis stabilizer comprises a glycidyl ether epoxy compound.
[0027] Preferably, the glycidyl ether epoxy compound includes any one of phenyl glycidyl ether, bisphenol A diglycidyl ether or tetrakis(phenylglycidyl)ethane, or a combination of at least two thereof.
[0028] In the present invention, the addition of a specific hydrolysis inhibitor can utilize the imine group or epoxy group to react with the terminal carboxyl group to generate a stable ureide structure or ring-opening polymerization, consume the number of terminal carboxyl groups of PLA, delay the decrease of pH value in the environment, and thus effectively inhibit the hydrolysis of PLA.
[0029] Preferably, the mass ratio of the compatibilizer, toughening agent and hydrolysis inhibitor is (4-8):(10-14):3, for example, it can be 4:10:3, 4:12:3, 4:14:3, 6:10:3, 2:3:1, 6:14:3, 8:10:3, 8:12:3 or 8:14:3, etc.
[0030] In a second aspect, the present invention provides a method for preparing the environmentally friendly and degradable PC / PLA alloy composition as described in the first aspect, the preparation method comprising:
[0031] PC, PLA, a compatibilizer, a toughening agent and a hydrolysis inhibitor are mixed and melt co-extruded to obtain the environmentally friendly and degradable PC / PLA alloy composition.
[0032] Preferably, the mixing time is 9-18 min, for example, it can be 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min or 18 min.
[0033] Preferably, the melt coextrusion is performed by a twin-screw extruder.
[0034] Preferably, the rotation speed of the twin-screw extruder is 450-550r / min, for example, it can be 455r / min, 460r / min, 470r / min, 480r / min, 490r / min, 500r / min, 510r / min, 520r / min, 530r / min, 540r / min or 545r / min, etc.
[0035] Preferably, the temperature of the twin-screw extruder includes:
[0036] The temperature of zone one is 50-105°C (for example, it can be 50°C, 60°C, 70°C, 80°C, 90°C, 100°C or 105°C, etc.), the temperature of zone two is 220-240°C (for example, it can be 220°C, 225°C, 230°C, 235°C or 240°C, etc.), the temperature of zone three is 220-240°C (for example, it can be 220°C, 225°C, 230°C, 235°C or 240°C, etc.), the temperature of zone four is 225-245°C (for example, it can be 225°C, 230°C, 235°C, 240°C or 245°C, etc.), the temperature of zone five is 225-245°C (for example, it can be 225°C, 230°C, 235°C, 240°C or 245°C, etc.), and the temperature of zone six is 225-245°C (for example, it can be 22 The temperature of zone 7 is 225-245°C (for example, it can be 225°C, 230°C, 235°C, 240°C or 245°C, etc.), the temperature of zone 8 is 225-245°C (for example, it can be 225°C, 230°C, 235°C, 240°C or 245°C, etc.), the temperature of zone 9 is 225-245°C (for example, it can be 225°C, 230°C, 235°C, 240°C or 245°C, etc.), the temperature of zone 10 is 230-250°C (for example, it can be 230°C, 235°C, 240°C, 245°C or 250°C, etc.), and the temperature of zone 11 is 230-250°C (for example, it can be 230°C, 235°C, 240°C, 245°C or 250°C, etc.).
[0037] In a third aspect, the present invention provides an environmentally friendly and degradable PC / PLA alloy material, wherein the environmentally friendly and degradable PC / PLA alloy material comprises the environmentally friendly and degradable PC / PLA alloy composition described in the first aspect.
[0038] In a fourth aspect, the present invention provides an application of the environmentally friendly and degradable PC / PLA alloy material as described in the third aspect in food or drug packaging, textiles or medical products.
[0039] Furthermore, the environmentally friendly and degradable PC / PLA alloy material provided by the present invention can also be widely used in the production of high-end electronic and electrical components such as notebooks and mobile phones, as well as automotive interior parts and mechanical components.
[0040] Compared with the prior art, the present invention has at least the following beneficial effects:
[0041] The present invention can effectively improve the compatibility of PC / PLA by selecting and compounding specific components, thereby obtaining a high-toughness PC / PLA alloy composition, and further obtaining an environmentally friendly and degradable PC / PLA alloy material with strong impact resistance, which has good application prospects. DETAILED DESCRIPTION
[0042] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0043] Some of the raw material information involved in the following implementation is as follows:
[0044] PC: Makrolon 2405, Makrolon 2407, Makrolon 3100 purchased from Bayer, Germany;
[0045] PLA: purchased from the United States RTP 2099X, RTP 126218C;
[0046] Styrene-Acrylonitrile-Glycidyl Methacrylate (SAG): purchased from Nantong Rizhishengsheng Molecular New Materials Technology Co., Ltd., SAG001;
[0047] Acrylonitrile Butadiene Styrene (ABS): purchased from Chi Mei Industrial Co., Ltd. ABS PA-757K;
[0048] MBS: purchased from Rohm and Haas, EXL-2690;
[0049] ACR: purchased from Mitsubishi Chemical Corporation, Japan, C223A;
[0050] Polycarbodiimide (PCDI): purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., A298745, molecular weight 4000, analytical grade, purity ≥95%;
[0051] 1,4-Butanediol diglycidyl ether: the epoxy value is 0.80-0.83eq / 100g, purchased from Hubei Siweitu New Material Technology Co., Ltd.
[0052] Example 1
[0053] This embodiment provides an environmentally friendly and degradable PC / PLA alloy composition, and the raw materials for preparing the composition include the following components in weight percentage:
[0054]
[0055]
[0056] The preparation method of the environmentally friendly and degradable PC / PLA alloy composition is as follows:
[0057] Makrolon 2405, SAG, MBS and PCDI were added into a high-speed mixer and mixed evenly for 13 minutes to obtain a PC mixture. The PC mixture and RTP 2099X were added into the main feeder of a twin-screw extruder respectively for melt co-extrusion. The extruder temperature was as follows: the temperature of zone 1 was 100° C., the temperature of zone 2 was 230° C., the temperature of zone 3 was 230° C., the temperature of zone 4 was 235° C., the temperature of zone 5 was 235° C., the temperature of zone 6 was 240° C., the temperature of zone 7 was 240° C., the temperature of zone 8 was 240° C., the temperature of zone 9 was 240° C., the temperature of zone 10 was 240° C., the temperature of zone 11 was 235° C., the screw speed of the twin-screw extruder was 500 r / min, and after extrusion by the screw extruder, the mixture was cooled, blow-dried and pelletized to obtain the environmentally friendly and degradable PC / PLA alloy composition.
[0058] Example 2
[0059] This embodiment provides an environmentally friendly and degradable PC / PLA alloy composition, and the raw materials for preparing the composition include the following components in weight percentage:
[0060]
[0061] The preparation method of the environmentally friendly and degradable PC / PLA alloy composition is as follows:
[0062] Makrolon 2407, SAG, MBS and 1,4-butanediol diglycidyl ether were added into a high-speed mixer and mixed evenly for 9 minutes to obtain a PC mixture. The PC mixture and RTP 126218C were respectively added from the main feeder of a twin-screw extruder for melt co-extrusion. The extruder temperatures were as follows: the temperature of zone 1 was 105°C, the temperature of zone 2 was 240°C, the temperature of zone 3 was 240°C, the temperature of zone 4 was 245°C, the temperature of zone 5 was 245°C, the temperature of zone 6 was 245°C, the temperature of zone 7 was 245°C, the temperature of zone 8 was 245°C, the temperature of zone 9 was 245°C, the temperature of zone 10 was 250°C, the temperature of zone 11 was 250°C, the screw speed of the twin-screw extruder was 550r / min, and after extrusion by the screw extruder, the extruder was cooled, blow-dried and pelletized to obtain the environmentally friendly and degradable PC / PLA alloy composition.
[0063] Example 3
[0064] This embodiment provides an environmentally friendly and degradable PC / PLA alloy composition, and the raw materials for preparing the composition include the following components in weight percentage:
[0065]
[0066] The preparation method of the environmentally friendly and degradable PC / PLA alloy composition is as follows:
[0067] Makrolon 3100, SAG, ACR and PCDI were added into a high-speed mixer and mixed evenly for 18 minutes to obtain a PC mixture. The PC mixture and RTP 2099X were added into the main feeder of a twin-screw extruder respectively for melt co-extrusion. The extruder temperature was as follows: the temperature of zone 1 was 50°C, the temperature of zone 2 was 220°C, the temperature of zone 3 was 220°C, the temperature of zone 4 was 225°C, the temperature of zone 5 was 225°C, the temperature of zone 6 was 225°C, the temperature of zone 7 was 225°C, the temperature of zone 8 was 225°C, the temperature of zone 9 was 225°C, the temperature of zone 10 was 230°C, the temperature of zone 11 was 230°C, the screw speed of the twin-screw extruder was 450r / min, and after extrusion by the screw extruder, the extruder was cooled, blow-dried and pelletized to obtain the environmentally friendly and degradable PC / PLA alloy composition.
[0068] Example 4
[0069] This embodiment provides an environmentally friendly and degradable PC / PLA alloy composition, and the raw materials for preparing the composition include the following components in weight percentage:
[0070]
[0071] The preparation method of the environmentally friendly and degradable PC / PLA alloy composition is the same as that in Example 1.
[0072] Example 5
[0073] This embodiment provides an environmentally friendly and degradable PC / PLA alloy composition, and the raw materials for preparing the composition include the following components in weight percentage:
[0074]
[0075] The preparation method of the environmentally friendly and degradable PC / PLA alloy composition is the same as that in Example 1.
[0076] Example 6
[0077] This embodiment provides an environmentally friendly and degradable PC / PLA alloy composition, and the raw materials for preparing the composition include the following components in weight percentage:
[0078]
[0079]
[0080] The preparation method of the environmentally friendly and degradable PC / PLA alloy composition is the same as that in Example 1.
[0081] Example 7
[0082] This embodiment provides an environmentally friendly and degradable PC / PLA alloy composition, and the raw materials for preparing the composition include the following components in weight percentage:
[0083]
[0084] The preparation method of the environmentally friendly and degradable PC / PLA alloy composition is the same as that in Example 1.
[0085] Example 8
[0086] This embodiment provides an environmentally friendly and degradable PC / PLA alloy composition, and the raw materials for preparing the composition include the following components in weight percentage:
[0087]
[0088] The preparation method of the environmentally friendly and degradable PC / PLA alloy composition is the same as that in Example 1.
[0089] Example 9
[0090] This embodiment provides an environmentally friendly and degradable PC / PLA alloy composition, and the raw materials for preparing the composition include the following components in weight percentage:
[0091]
[0092] The preparation method of the environmentally friendly and degradable PC / PLA alloy composition is the same as that in Example 1.
[0093] Example 10
[0094] This embodiment provides an environmentally friendly and degradable PC / PLA alloy composition, which differs from Example 5 in that the SAG content of 4wt% is adjusted to 3.5wt%, and the PCDI content of 2wt% is adjusted to 2.5wt%. Other components, contents and preparation methods are the same as those in Example 5.
[0095] Embodiment 11
[0096] This embodiment provides an environmentally friendly and degradable PC / PLA alloy composition, which differs from Example 5 in that the SAG content of 4wt% is adjusted to 3.35wt%, the MBS content of 8wt% is adjusted to 8.25wt%, and the PCDI content of 2wt% is adjusted to 2.4wt%. Other components, contents and preparation methods are the same as those in Example 5.
[0097] Example 12
[0098] This embodiment provides an environmentally friendly and degradable PC / PLA alloy composition, which differs from Example 5 in that the SAG content of 4wt% is adjusted to 4.48wt%, the MBS content of 8wt% is adjusted to 7.84wt%, and the PCDI content of 2wt% is adjusted to 1.68wt%. The other components, contents and preparation methods are the same as those in Example 5.
[0099] Embodiment 13
[0100] This embodiment provides an environmentally friendly and degradable PC / PLA alloy composition, which differs from Example 5 in that the content of MBS is adjusted from 8wt% to 8.32wt%, and the content of PCDI is adjusted from 2wt% to 1.68wt%. Other components, contents and preparation methods are the same as those in Example 5.
[0101] Embodiment 14
[0102] This embodiment provides an environmentally friendly and degradable PC / PLA alloy composition, which is different from Example 1 only in that SAG is replaced by ABS, and other components, contents and preparation methods are the same as those in Example 1.
[0103] Comparative Example 1
[0104] This comparative example provides a PC / PLA alloy composition, which differs from Example 1 in that SAG is not added, and its reduced content is proportionally distributed to MBS and PCDI, and other components, contents and preparation methods are the same as those in Example 1.
[0105] Comparative Example 2
[0106] This comparative example provides a PC / PLA alloy composition, which differs from Example 1 in that MBS is not added, and its reduced content is proportionally distributed to SAG and PCDI, and other components, contents and preparation methods are the same as those in Example 1.
[0107] Comparative Example 3
[0108] This comparative example provides a PC / PLA alloy composition, which differs from Example 1 in that PCDI is not added, and its reduced content is proportionally distributed to SAG and MBS, and other components, contents and preparation methods are the same as those in Example 1.
[0109] Comparative Example 4
[0110] This comparative example provides a PC / PLA alloy composition, the raw materials for its preparation include the following components in weight percentage:
[0111]
[0112] The preparation method of the PC / PLA alloy composition is the same as that of Example 1.
[0113] Comparative Example 5
[0114] This comparative example provides a PC / PLA alloy composition, the raw materials for its preparation include the following components in weight percentage:
[0115]
[0116] The preparation method of the PC / PLA alloy composition is the same as that of Example 1.
[0117] Comparative Example 6
[0118] This comparative example provides a PC / PLA alloy composition, the raw materials for its preparation include the following components in weight percentage:
[0119]
[0120] The preparation method of the PC / PLA alloy composition is the same as that of Example 1.
[0121] The PC / PLA alloy compositions obtained in the above Examples 1-14 and Comparative Examples 1-6 were subjected to performance tests, and the test methods or standards were as follows:
[0122] (1) Tensile strength test: Test according to the test method provided in ISO-527-2012;
[0123] (2) Flexural modulus test: Test according to the test method provided in ISO-178-2010;
[0124] (3) ISO room temperature and low temperature notched impact strength test: Test according to the test method provided in ISO-179-2010;
[0125] (4) ASTM 3.2mm room temperature and low temperature notched impact strength test, ASTM 6.4mm room temperature and low temperature notched impact strength test: Tested in accordance with the test method provided in ASTM D256-2010;
[0126] (5) Vicat softening point temperature test: Test according to the test method provided in ISO 306-2022;
[0127] (6) Melt index performance test: The test was conducted in accordance with the test method provided in ISO 1133-2011, with the test conditions being 260°C and 5 kg.
[0128] The test results are shown in Table 1.
[0129] Table 1
[0130]
[0131]
[0132] The test results show that:
[0133] (1) It can be seen from Examples 1-14 that the present invention can achieve compatibility of PC and PLA when mixed through the synergistic effect of specific compatibilizers, toughening agents and hydrolysis inhibitors, thereby obtaining a high-toughness, impact-resistant and environmentally friendly degradable PC / PLA alloy composition; further, through the specific selection of each component and its content, the obtained environmentally friendly degradable PC / PLA alloy composition can ensure good tensile strength and flexural modulus while also having good impact resistance, that is, its ISO room temperature and low temperature notched impact strength, ASTM 3.2mm room temperature and low temperature notched impact strength and ASTM 6.4mm room temperature and low temperature notched impact strength can simultaneously reach a high level.
[0134] (2) By comparing Example 5 with Examples 10-13, it can be seen that when the mass ratio of the specific compatibilizer, toughening agent and hydrolysis inhibitor in the present invention is (4-8):(10-14):3, the obtained environmentally friendly and degradable PC / PLA alloy composition has a better technical effect. When it exceeds this range, its impact resistance is reduced.
[0135] (3) By comparing Example 1 with Example 14, it can be seen that, compared with PC / ABS, the selection of the specific compatibilizer in the present invention can significantly improve the impact resistance of the obtained environmentally friendly and degradable PC / PLA alloy composition.
[0136] (4) By comparing Example 1 with Comparative Examples 1-3, it can be seen that the present invention can exert a synergistic effect through the compounding of the compatibilizer, the toughening agent and the hydrolysis inhibitor, so that the obtained environmentally friendly and degradable PC / PLA alloy composition has high toughness and thus has excellent impact resistance.
[0137] (5) By comparing Example 1 with Comparative Examples 4-6, it can be seen that the present invention can improve the impact resistance of the obtained environmentally friendly and degradable PC / PLA alloy composition by specifically selecting the content of each component.
[0138] In summary, the present invention can effectively improve the compatibility of PC / PLA through the selection and compounding of specific combinations, thereby obtaining a high-toughness PC / PLA alloy composition, and then obtaining an environmentally friendly and degradable PC / PLA alloy material with strong impact resistance, which has a good application prospect.
[0139] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. An environmentally friendly and degradable PC / PLA alloy composition, characterized in that: The raw materials for preparing the environmentally friendly and degradable PC / PLA alloy composition include the following components in weight percentage:
2. The environmentally friendly and degradable PC / PLA alloy composition according to claim 1, characterized in that: The PC comprises aromatic polycarbonate; Preferably, the aromatic polycarbonate comprises at least 70% aromatic moieties; Preferably, the PC comprises bisphenol A polycarbonate; Preferably, the weight average molecular weight of the PC is 15,000-40,000.
3. The environmentally friendly and degradable PC / PLA alloy composition according to claim 1 or 2, characterized in that: The PLA includes any one of L-polylactic acid, D-polylactic acid, epoxy-modified polylactic acid or maleic anhydride-modified polylactic acid or a combination of at least two thereof; Preferably, the weight average molecular weight of the PLA is 15000-25000.
4. The environmentally friendly and degradable PC / PLA alloy composition according to any one of claims 1 to 3, characterized in that: The compatibilizer is an epoxy compatibilizer; Preferably, the compatibilizer is styrene-acrylonitrile-glycidyl methacrylate.
5. The environmentally friendly and degradable PC / PLA alloy composition according to any one of claims 1 to 4, characterized in that: The toughening agent is a core-shell toughening agent; Preferably, the core-shell toughening agent includes any one of C-223A, AX8900, S2100, BTA731, ACR, and MBS, or a combination of at least two thereof.
6. The environmentally friendly and degradable PC / PLA alloy composition according to any one of claims 1 to 5, characterized in that: The hydrolysis inhibitor includes a diimine-type hydrolysis inhibitor and / or an epoxy compound hydrolysis stabilizer; Preferably, the diimide-type hydrolysis inhibitor comprises monocarbodiimide and / or polycarbodiimide; Preferably, the epoxy compound hydrolysis stabilizer comprises a glycidyl ether epoxy compound; Preferably, the glycidyl ether epoxy compound includes any one of phenyl glycidyl ether, bisphenol A diglycidyl ether or tetrakis(phenylglycidyl)ethane, or a combination of at least two thereof.
7. The environmentally friendly and degradable PC / PLA alloy composition according to any one of claims 1 to 6, characterized in that: The mass ratio of the compatibilizer, toughening agent and hydrolysis inhibitor is (4-8):(10-14):
3.
8. A method for preparing the environmentally friendly and degradable PC / PLA alloy composition according to any one of claims 1 to 7, characterized in that: The preparation method comprises: Mixing PC, PLA, a compatibilizer, a toughening agent and a hydrolysis inhibitor, and melt co-extruding to obtain the environmentally friendly and degradable PC / PLA alloy composition; Preferably, the mixing time is 9-18 min; Preferably, the melt coextrusion is carried out by a twin-screw extruder; Preferably, the speed of the twin-screw extruder is 450-550r / min; Preferably, the temperature of the twin-screw extruder includes: The temperature of zone one is 50-105℃, the temperature of zone two is 220-240℃, the temperature of zone three is 220-240℃, the temperature of zone four is 225-245℃, the temperature of zone five is 225-245℃, the temperature of zone six is 225-245℃, the temperature of zone seven is 225-245℃, the temperature of zone eight is 225-245℃, the temperature of zone nine is 225-245℃, the temperature of zone ten is 230-250℃, and the temperature of zone eleven is 230-250℃.
9. An environmentally friendly and degradable PC / PLA alloy material, characterized in that: The environmentally friendly and degradable PC / PLA alloy material comprises the environmentally friendly and degradable PC / PLA alloy composition according to any one of claims 1 to 7.
10. Use of the environmentally friendly and degradable PC / PLA alloy material as claimed in claim 9 in food or drug packaging, textiles or medical products.