Formula and preparation process of plastic particles for processing shells of electrical products

By using a combination of modified flat glass fiber and flame retardant, the problem of degradation of flame retardant performance between glass fiber and PA66 material during combustion is solved, and the flame retardant and mechanical properties of composite materials are improved, which is suitable for processing of electrical product shells.

CN119081400AInactive Publication Date: 2024-12-06ZHEJIANG HENGMEI NEW MATERIALS CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411599192.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-11
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Glass fiber and PA66 materials cause flame retardant performance to decline during combustion, which cannot meet the material requirements in the electrical field. At the same time, the poor compatibility of the two affects the appearance of the product.

Method used

Flat glass fibers are used to replace round-section glass fibers, and modified by silane coupling agents, combined with antioxidants, lubricants, flame retardants and voltage stabilizers, to prepare excellent mechanical strength, insulation and flame retardant Plastic particles improve the distribution and compatibility of fibers in composite materials.

Benefits of technology

It significantly improves the flame retardant properties and mechanical properties of composite materials, enhances the compatibility of glass fibers with PA66, ensures the safety and performance of electrical product shells, and is suitable for the preparation of electrical circuit breaker materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081400A_ABST
    Figure CN119081400A_ABST
Patent Text Reader

Abstract

The invention discloses a formula and a preparation process of plastic particles for electrical product shell processing, and relates to the technical field of functional plastics, the formula of the plastic particles for electrical product shell processing comprises, by weight, 60-90 parts of PA66, 10-40 parts of modified glass fiber, 0.1-0.6 part of an antioxidant, 0.2-1 part of a lubricant, and 10-20 parts of a flame retardant. By modifying the glass fiber, the compatibility of the glass fiber and the PA66 is increased, the mechanical property and the insulating property of a final product are enhanced together with aromatic voltage stabilizers contained in the other auxiliaries, meanwhile, the special structure of the flat glass fiber is utilized, a combination of the flat glass fiber and the flame retardant is used, and the flame retardant property of the product is improved. The defect that a PA66 product is poor in flame retardant property is overcome, functional plastic particles with high comprehensive performance are obtained, and the plastic particles meet the requirements for manufacturing shells of electrical products such as circuit breaker shells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of functional plastics, and in particular to a formula and a preparation process of plastic particles used for processing housings of electrical products. Background Art

[0002] Plastic particles are the common name for plastic particles. They are the raw materials for storage, transportation and processing of plastics in the form of semi-finished products. Plastic particles are often placed in an injection molding machine, heated and melted, and the molten plastic is added to the mold and cooled to form. The molded plastic model has the same properties as the plastic particles. Therefore, plastic particles with different functional properties are continuously researched and developed, playing an important role in various fields.

[0003] Polyamide (PA), as a kind of thermoplastic engineering plastics, also known as nylon, has the characteristics of large output, wide variety, wide application and excellent performance. Specifically, PA plastic has high tensile strength and compressive strength, as well as good wear resistance and self-lubrication, and can resist the erosion of various chemicals. Among them, PA6 and PA66 have the largest output and consumption. PA66 has the characteristics of corrosion resistance, easy processing and wear resistance, but it is a flammable material. Through flame retardant and other modification operations, the flame retardancy and heat resistance of PA66 can be enhanced, thereby meeting the material requirements of the electrical field.

[0004] Glass fiber modified PA material can improve the tensile strength and volume resistivity of the composite material. However, the addition of glass fiber makes it difficult to extinguish the flame of PA66 material due to the wick effect during the combustion process, and the flame retardant performance is significantly reduced, which cannot meet the flame retardant requirements of the material. Compared with traditional round-section glass fiber, flat glass fiber, as a new type of glass fiber with a special structure, has unique advantages in warping resistance and processing fluidity. However, both round-section glass fiber and flat glass fiber have poor compatibility with plastic polymers such as PA66, which affects the appearance of the product.

[0005] The combination of glass fiber and PA66 enhances the tensile strength and insulation of PA66 composite materials, but reduces the flame retardancy. Further modification operations can be performed to enhance the flame retardancy of the composite materials so that they can meet the requirements of materials in the electrical field. Summary of the invention

[0006] The present invention is made in view of the above-mentioned problems, and its purpose is to provide a formula and preparation process of plastic particles for processing electrical product casings. By using flat glass fibers instead of round-section glass fibers, the plastic particles not only have excellent mechanical strength and insulation, but the orientation degree of the glass fibers in the composite material is significantly lower, the surface area with higher order orientation accounts for a smaller proportion, the fiber aggregation phenomenon in the core layer is lighter, the overall distribution is uniform, and the orientation degree of the fibers in the core layer is also lower, ultimately exhibiting excellent flame retardancy.

[0007] The technical solution adopted by the present invention is as follows: In a first aspect, the present invention provides a formula of plastic particles for processing electrical product housings, wherein the raw materials include the following components by weight: 60-90 parts of PA66, 10-40 parts of modified glass fiber, 0.1-0.6 parts of antioxidant, 0.2-1 parts of lubricant, 10-20 parts of flame retardant, and 2-5 parts of other additives.

[0008] Furthermore, the modified glass fiber includes modified round-section glass fiber and modified flat glass fiber.

[0009] Furthermore, the modification method of the modified glass fiber is: silane coupling agent: deionized water: anhydrous ethanol are mixed in a mass ratio of 1:30:30 to prepare a modified solution, and the modified solution is added in a ratio of 10 ml per 1g of glass fiber. After fully stirring for 10-20 minutes, ultrasonically treated for 1-2 hours, taken out and dried in a constant temperature drying oven at 100 degrees Celsius for 6-8 hours to obtain the modified glass fiber.

[0010] Furthermore, the antioxidant includes antioxidant 168 and antioxidant 1098, and the antioxidant 168 and antioxidant 1098 are mixed in a ratio of 1:1.

[0011] Furthermore, the lubricant is ethylene bisstearamide, which also serves as a dispersant.

[0012] Furthermore, the flame retardant is an organophosphorus flame retardant.

[0013] Furthermore, the other auxiliary agents include a voltage stabilizer and silica sol, and the voltage stabilizer includes a sterically hindered piperidine free radical scavenger and an organic stabilizing substance.

[0014] Furthermore, the organic stabilizing substance contains ortho-phenolic hydroxyl groups and ethylene oxide side chains.

[0015] In a second aspect, the present invention further provides a process for preparing plastic particles for use in processing electrical product housings.

[0016] The steps include: (1) Place PA66 in a constant temperature drying oven and dry it for 4-5 hours. The temperature of the constant temperature drying oven is set at 75-85 degrees Celsius. (2) Take out the PA66 from the constant temperature drying oven, weigh the corresponding mass together with the other raw materials, add them into the twin-screw extruder according to the proportion, and carry out heating and melting, plasticizing and mixing, cooling and solidification, extrusion granulation, separation and screening, and anti-static packaging and storage operations; (3) Dry the obtained plastic particles in a constant temperature drying oven at 100 degrees Celsius for 5-6 hours, and then form standard specimens using an injection molding machine; (4) Take out the prepared standard specimen and let it stand for 24 hours before measuring the material indicators.

[0017] Furthermore, the process parameters of the twin-screw extruder are: The temperature in zone 1 is 140-160 degrees Celsius, the temperature in zone 2 is 270-280 degrees Celsius, the temperature in zone 3 is 270-280 degrees Celsius; the temperature in zone 4 is 260-270 degrees Celsius; the temperature in zone 5 is 260-270 degrees Celsius; the temperature in zone 6 is 250-270 degrees Celsius; the temperature in zone 7 is 255-270 degrees Celsius; the temperature in zone 8 is 260-270 degrees Celsius; the temperature in zone 9 is 260-270 degrees Celsius; The head temperature is 265 degrees Celsius; the vacuum degree is 0.04-0.06 MPa; the main engine speed is 700-750 r / min; the feeding speed is 420-450 r / min; and the pelletizing speed is 400-650 r / min.

[0018] Furthermore, the process parameters of the injection molding machine are: The temperature of zone 1 is 270 degrees Celsius; the temperature of zone 2 is 260 degrees Celsius; the temperature of zone 3 is 260 degrees Celsius; the temperature of zone 4 is 260 degrees Celsius; the temperature of zone 5 is 265 degrees Celsius; the injection pressure is 60-80 MPa; the injection speed is 35-45cm 3 / s, injection time is 26s.

[0019] Furthermore, the material indicators include material density, mechanical properties, flame retardant properties and insulation properties.

[0020] Furthermore, the mechanical properties include tensile strength, flexural strength, flexural modulus and notched impact strength.

[0021] Furthermore, the flame retardant performance includes vertical combustion performance and horizontal combustion performance.

[0022] Furthermore, the insulation properties include breakdown strength, dielectric constant and volume resistivity.

[0023] The beneficial effects of the present invention are: (1) The plastic particles prepared by the present invention for processing electrical product housings overcome the disadvantage of poor flame retardancy of PA66 by modifying PA66 with glass fibers and utilizing the special structure of flat glass fibers in combination with flame retardants.

[0024] (2) The plastic particles prepared by the present invention for processing electrical product shells modify glass fibers, thereby enhancing the compatibility between glass fibers and plastic polymers and enhancing the mechanical properties and insulation properties of PA66.

[0025] (3) The present invention prepares a plastic particle for processing the outer shell of an electrical product. An aromatic voltage stabilizer is introduced into the raw material. The aromatic voltage stabilizer is used to suppress the growth of electrical dendrites from two aspects by inhibiting the scavenging of free radicals and stabilizing the crystal structure of the material, thereby reducing the defects between the lamellae.

[0026] (4) The plastic particles prepared by the present invention for processing electrical product shells have excellent product performance and significant reprocessing capacity, and can be used in the preparation of electrical circuit breaker materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a process flow chart of preparing plastic particles for electrical product housing processing according to the present invention; Figure 2 The present invention is a scanning electron microscope image of a plastic particle used for processing an electrical product housing. DETAILED DESCRIPTION

[0028] The following is a detailed description of embodiments of the present invention, but the present invention can be implemented in many different ways as defined and covered by the claims.

[0029] Example 1 A formula of plastic particles for processing electrical product housings: PA66 70 parts, modified glass fiber 30 parts, antioxidant 0.3 parts, lubricant 0.5 parts, flame retardant 18 parts, other additives 3 parts.

[0030] Furthermore, the modified glass fiber is a modified flat glass fiber.

[0031] Furthermore, the modification method of the modified glass fiber is as follows: silane coupling agent: deionized water: anhydrous ethanol are mixed in a mass ratio of 1:30:30 to prepare a modified solution, the modified solution is added in a ratio of 10 ml per 1 g of glass fiber, fully stirred for 12 minutes, ultrasonicated for 1.5 hours, and then taken out and dried in a constant temperature drying oven at 100 degrees Celsius for 6 hours to obtain modified glass fiber. Compared with the unmodified glass fiber, the compatibility between the modified glass fiber and the PA66 plastic polymer is significantly enhanced.

[0032] Furthermore, the antioxidant includes 0.15 parts of antioxidant 168 and 0.15 parts of antioxidant 1098. The addition of antioxidants protects plastic products from being oxidized and aged by oxygen in the air, which is essential for maintaining the stability of the physical and chemical properties of plastic particles, thereby extending their service life and improving their use value. The addition of antioxidants can also improve the processing properties of plastics, making plastic particles easier to shape in subsequent injection molding, extrusion and other processing processes, thereby improving production efficiency.

[0033] Furthermore, the lubricant is ethylene bisstearamide, which also acts as a dispersant. The polymer usually has a high viscosity after melting. The friction and adhesion between particles and between particles and equipment during processing will affect production efficiency and product quality. Ethylene bisstearamide can reduce these frictions and reduce the interfacial adhesion performance, making the plastic particles smoother during processing, and at the same time making the additives more evenly distributed in the plastic particles, preventing the particles from agglomerating, and playing the role of a dispersant.

[0034] Furthermore, the flame retardant is an organic phosphorus flame retardant, specifically a phosphate ester, which will undergo thermal decomposition at high temperatures, and water and acidic substances will be produced in the process. These decomposition products can dilute the air around the combustibles, and the released gases (such as ammonia, nitrogen, etc.) can isolate oxygen or dilute combustible gases, thereby reducing the speed and intensity of the combustion reaction. At high temperatures, the phosphate ester can cause the polymer surface to dehydrate and carbonize rapidly, forming a protective carbon layer. This carbon layer has good heat insulation and oxygen isolation functions, and can effectively prevent the combustibles from contacting the outside air, further reducing the possibility of combustion.

[0035] Furthermore, the other additives include a voltage stabilizer and silica sol, the voltage stabilizer includes a sterically hindered piperidine free radical scavenger and an organic stabilizing substance, the silica sol is used to enhance the bonding between PA66 particles, the sterically hindered piperidine free radical scavenger can absorb residual oxygen in the polymer, and the oxidized nitroxide free radicals can effectively inhibit the generation of macromolecular free radicals, which not only increases the starting voltage of the polymer electrical tree, inhibits the growth of the electrical tree, but also prolongs the insulation life of the polymer under a uniform electric field.

[0036] Furthermore, the organic stabilizing substance contains ortho-phenolic hydroxyl groups and ethylene oxide side chains, which can stabilize the crystal structure, reduce defects between crystal lamellae, moderate the electric field intensity near the needle tip, and inhibit the growth of electrical dendrites.

[0037] The preparation process is as follows: (1) Raw material preparation and pretreatment: PA66 is placed in a constant temperature drying oven for 4 hours. The temperature of the constant temperature drying oven is set to 80 degrees Celsius. PA66 itself has strong hygroscopicity and water sensitivity, and it is easy to absorb moisture in the air. Moisture will cause PA66 to degrade during the modification heating process. High temperature drying is conducive to ensuring the stability of the modified material performance. If PA66 contains too much water, bubbles and defects may be generated during the modification process, thereby affecting the quality and performance of the product; (2) Feeding and conveying: Take out the PA66 from the constant temperature drying oven and weigh the corresponding mass portions together with the other raw materials according to the proportion, and convey them to the feeding port of the twin-screw extruder through a screw feeder. The feeding speed is 420r / min; (3) Heating and melting: the raw material particles are heated and melted in the twin-screw extruder to form a uniform plastic melt. During this process, the main engine speed is 720 r / min; (4) Plasticizing and mixing: The threads on the screw shear, extrude, and convey the material. Under the combined action of heating and shearing force, the material gradually melts and plasticizes, and is fully mixed. The meshing structure of the twin screws helps to distribute and disperse the material; (5) Cooling and solidification: the material after plasticization and mixing is pushed to the die head, extruded through the specific hole pattern on the die to form a strip-shaped material, and then quickly cooled and solidified by underwater cooling; (6) Extrusion granulation, using a pelletizing device to cut the strip material into pellets of the required length; (7) Separation and screening: placing the cooled particles into a vibrating screening machine for screening and separation to obtain finished particles that meet the specifications; (8) Anti-static packaging and storage: Qualified finished particles are dried in a constant temperature drying oven at 100 degrees Celsius for 6 hours, and then blown by an ion fan for 5 minutes to remove static electricity. The treated plastic particles are packaged and stored in a dry and cool environment to prevent moisture and deterioration; (9) Randomly select product samples, dry them in a constant temperature drying oven at 100 degrees Celsius for 5 hours, and use an injection molding machine to make standard specimens. The length, width and height of the standard specimens are 80 mm × 10 mm × 4 mm respectively; (10) After the standard specimen is prepared, let it stand for 24 hours before measuring the material index.

[0038] Furthermore, the process parameters of the injection molding machine are: The temperature of zone 1 is 270 degrees Celsius; the temperature of zone 2 is 260 degrees Celsius; the temperature of zone 3 is 260 degrees Celsius; the temperature of zone 4 is 260 degrees Celsius; the temperature of zone 5 is 265 degrees Celsius; the injection pressure is 80MPa; the injection speed is 40cm 3 / s, injection time is 26s.

[0039] Furthermore, the material indicators include material density, mechanical properties, flame retardant properties and insulation properties.

[0040] Furthermore, the density test was carried out according to GB / T 1033.1-2008, and each sample was repeated 3 times to take the average value.

[0041] Furthermore, the mechanical properties include tensile strength, flexural strength, flexural modulus and notched impact strength. The tensile properties are tested in accordance with ISO 527.2-2012 "Plastics-Determination of tensile properties Part 2: Test conditions for molded and extruded plastics", and each sample is repeated 3 times to take the average value; the flexural properties are tested in accordance with ISO 178-2019 "Plastics-Determination of flexural properties", and each sample is repeated 3 times to take the average value; impact properties: tested in accordance with ISO 179.2-2020 "Plastics-Determination of impact properties of simply supported beams Part 2: Instrumented impact test", and each sample is repeated 8 times to take the average value.

[0042] Furthermore, the flame retardant properties include vertical burning properties and horizontal burning properties, which are tested in accordance with GB / T 2408-2021 "Horizontal and vertical methods for determination of burning properties of plastics", and each sample is repeated 3 times to take the average value.

[0043] Furthermore, the insulation properties include breakdown strength, dielectric constant and volume resistivity. The breakdown strength test under DC and AC electric fields is carried out in accordance with GB / T 7141-2008, with the voltage increased step by step at a rate of 1 kV / s until the sample is broken down. Each sample is repeated 3 times and the average value is taken; the dielectric constant test is carried out in accordance with GB / T 31838.6-2021, with a frequency range of 40~100 MHz and a test temperature of 25°C. Each sample is repeated 3 times and the average value is taken; the volume resistivity test is carried out in accordance with GB / T 1410-2006, with each sample repeated 3 times and the average value is taken.

[0044] Example 2 Compared with Example 1, the only difference in Example 2 is that the formula of the plastic particles is different: PA66 60 parts, modified glass fiber 40 parts, antioxidant 0.3 parts, lubricant 0.5 parts, flame retardant 18 parts, other additives 3 parts, the modified glass fiber is flat glass fiber.

[0045] The preparation process and other related parameters of this embodiment are consistent with those of embodiment 1.

[0046] Example 3 Compared with Example 1, the only difference in Example 3 is that the formula of the plastic particles is different: 80 parts of PA66, 20 parts of modified glass fiber, 0.3 parts of antioxidant, 0.5 parts of lubricant, 18 parts of flame retardant, and 3 parts of other additives. The modified glass fiber is a flat glass fiber.

[0047] The preparation process and other related parameters of this embodiment are consistent with those of embodiment 1.

[0048] Example 4 Compared with Example 1, the only difference in Example 4 is that the formula of the plastic particles is different: 90 parts of PA66, 10 parts of modified glass fiber, 0.3 parts of antioxidant, 0.5 parts of lubricant, 18 parts of flame retardant, and 3 parts of other additives. The modified glass fiber is a flat glass fiber.

[0049] The preparation process and other related parameters of this embodiment are consistent with those of embodiment 1.

[0050] Example 5 Compared with Example 1, the only difference in Example 5 is that the formula of the plastic particles is different: PA66 60 parts, modified glass fiber 40 parts, antioxidant 0.3 parts, lubricant 0.5 parts, flame retardant 18 parts, other additives 3 parts, the modified glass fiber is a round cross-section glass fiber.

[0051] The preparation process and other related parameters of this embodiment are consistent with those of embodiment 1.

[0052] Example 6 Compared with Example 1, the only difference in Example 6 is that the formula of the plastic particles is different: PA66 70 parts, modified glass fiber 30 parts, antioxidant 0.3 parts, lubricant 0.5 parts, flame retardant 18 parts, other additives 3 parts, the modified glass fiber is a round cross-section glass fiber.

[0053] The preparation process and other related parameters of this embodiment are consistent with those of embodiment 1.

[0054] Example 7 Compared with Example 1, the only difference in Example 7 is that the formula of the plastic particles is different: 80 parts of PA66, 20 parts of modified glass fiber, 0.3 parts of antioxidant, 0.5 parts of lubricant, 18 parts of flame retardant, and 3 parts of other additives, wherein the modified glass fiber is a round-section glass fiber.

[0055] The preparation process and other related parameters of this embodiment are consistent with those of embodiment 1.

[0056] Example 8 Compared with Example 1, the only difference in Example 8 is that the formula of the plastic particles is different: 90 parts of PA66, 10 parts of modified glass fiber, 0.3 parts of antioxidant, 0.5 parts of lubricant, 18 parts of flame retardant, and 3 parts of other additives. The modified glass fiber is a round-section glass fiber.

[0057] The preparation process and other related parameters of this embodiment are consistent with those of embodiment 1.

[0058] Example 9 Compared with Example 1, the only difference in Example 9 is that the formula of the plastic particles is different: 70 parts of PA66, 30 parts of modified glass fiber, 0.3 parts of antioxidant, 0.5 parts of lubricant, 10 parts of flame retardant, and 3 parts of other additives. The modified glass fiber is a flat glass fiber.

[0059] The preparation process and other related parameters of this embodiment are consistent with those of embodiment 1.

[0060] Example 10 Compared with Example 1, the only difference in Example 10 is that the formula of the plastic particles is different: PA66 70 parts, modified glass fiber 30 parts, antioxidant 0.3 parts, lubricant 0.5 parts, flame retardant 18 parts, other additives 2 parts, the modified glass fiber is flat glass fiber.

[0061] The preparation process and other related parameters of this embodiment are consistent with those of embodiment 1.

[0062] Comparative Example 1 Compared with Example 1, the only difference in Comparative Example 1 is that the formula of the plastic particles is different: PA66 70 parts, modified glass fiber 0 parts, antioxidant 0.3 parts, lubricant 0.5 parts, flame retardant 18 parts, other additives 3 parts.

[0063] The preparation process and other related parameters of this embodiment are consistent with those of embodiment 1.

[0064] Comparative Example 2 Compared with Example 1, the only difference in Comparative Example 2 is that the formula of the plastic particles is different: PA66 70 parts, modified glass fiber 30 parts, antioxidant 0.3 parts, lubricant 0.5 parts, flame retardant 0 parts, other additives 3 parts, the modified glass fiber is flat glass fiber.

[0065] The preparation process and other related parameters of this embodiment are consistent with those of embodiment 1.

[0066] Comparative Example 3 Compared with Example 1, the only difference in Comparative Example 3 is that the formula of the plastic particles is different: PA66 70 parts, modified glass fiber 30 parts, antioxidant 0.3 parts, lubricant 0.5 parts, flame retardant 18 parts, other additives 0 parts, the modified glass fiber is flat glass fiber.

[0067] The preparation process and other related parameters of this embodiment are consistent with those of embodiment 1.

[0068] Comparative Example 4 Compared with Example 1, the only difference in Comparative Example 4 is that the formula of the plastic particles is different: PA66 70 parts, modified glass fiber 0 parts, antioxidant 0.3 parts, lubricant 0.5 parts, flame retardant 0 parts, other additives 3 parts, the modified glass fiber is flat glass fiber.

[0069] Comparative Example 5 Compared with Example 1, the only difference in Comparative Example 5 is that the formula of the plastic particles is different: 50 parts of PA66, 50 parts of modified glass fiber, 0.3 parts of antioxidant, 0.5 parts of lubricant, 18 parts of flame retardant, and 3 parts of other additives. The modified glass fiber is a flat glass fiber.

[0070] The preparation process and other related parameters of this embodiment are consistent with those of embodiment 1.

[0071] Comparative Example 6 Compared with Example 1, the only difference in Comparative Example 5 is that the formula of the plastic particles is different: 70 parts of PA66, 30 parts of unmodified glass fiber, 0.3 parts of antioxidant, 0.5 parts of lubricant, 18 parts of flame retardant, and 3 parts of other additives, wherein the unmodified glass fiber is a flat glass fiber.

[0072] The preparation process and other related parameters of this embodiment are consistent with those of embodiment 1.

[0073] Table 1 Composite material density and mechanical properties test data Note: Unless otherwise supplemented, the glass fibers mentioned in this article are all modified glass fibers.

[0074] Combining the data of Example 1 with that of Comparative Example 6, it can be seen that after the flat glass fiber is modified, the density and mechanical properties of the composite material are slightly enhanced. Combining the data of Examples 1 to 8, it can be seen that whether it is round-section glass fiber or flat glass fiber, the type of glass fiber has almost no effect on the density and mechanical properties of the composite material; Combining the data of Examples 1 to 10 with Comparative Examples 1 to 4, it can be seen that the proportion of glass fiber has a great influence on the mechanical properties of the material: when the glass fiber content is 30 parts and the PA66 content is 70 parts, the comprehensive mechanical properties are the best, and the density is The highest, the mechanical properties show a rule of first strengthening and then weakening with the change of the relative content of glass fiber. The addition of flame retardants has almost no effect on the density and mechanical properties. The addition of other additives will increase the density and mechanical properties of the material to a certain extent. The silica sol included in other additives has an ion particle size of nanometer level, a large specific surface area, low viscosity, good dispersibility and permeability. When modified and mixed, it penetrates the gaps of PA66 molecules. After mixing, the silica sol will firmly adhere to the surface of the object, thereby enhancing the bonding between the plastic particles, and then improving the density and mechanical properties of the composite material.

[0075] Table 2 Flame retardant properties test data of composite materials Combining the data of Example 1, Example 9, Comparative Example 1 and Comparative Example 4, it can be seen that the flame retardant promotes the flame retardant properties of the composite material; combining the data of Comparative Example 2 and Comparative Example 4, it can be seen that the flat glass fiber slightly enhances the flame retardant properties of the composite material; combining the data of Example 1, Example 10 and Comparative Example 3, it can be seen that other additives have almost no effect on the flame retardant properties of the composite material; combining all the data of Example 1-Example 10 and Comparative Example 1-Comparative Example 6, it can be seen that the round-section glass reduces the flame retardant properties of the composite material, and the combination of the round-section glass and the flame retardant still slightly reduces the flame retardant properties of the composite material. Flat glass fiber and flame retardant alone have limited effect on enhancing the flame retardant properties of composite materials. The combination of unmodified flat glass fiber and flame retardant improves the flame retardant properties of composite materials better than the effect of adding either alone, but it is still limited. However, the combination of modified flat glass fiber and flame retardant greatly enhances the flame retardant properties. When the glass fiber is flat glass fiber and its content is 30 parts and the PA66 content is 70 parts, the flame retardant properties of the composite material are the best. However, when the glass fiber is flat glass fiber and its content is 50 parts and the PA66 content is 50 parts, the enhancement effect on the flame retardant properties of the composite material is greatly reduced.

[0076] Table 3 Composite material insulation performance test data Combining the data of Example 1 and Comparative Example 6, it can be seen that the flat glass fiber has a certain promoting effect on the insulation performance of the composite material after modification. Combining the data of Example 1, Example 6, Comparative Example 1, Comparative Example 2 and Comparative Example 4, it can be seen that the glass fiber can greatly increase the insulation performance of the composite material. Combining the data of Example 1-Example 8, it can be seen that whether it is round-section glass fiber or flat glass fiber, the type of glass fiber has almost no effect on the insulation performance of the composite material, and when the glass fiber content is 20 parts, the PA66 content is 80 parts, and the glass fiber content is 30 parts, and the PA66 content is 70 parts, the insulation performance of the composite material of these two combinations is the best; Combining the data of Example 1, Example 10 and Comparative Example 3, it can be seen that other additives slightly increase the breakdown strength, but have almost no effect on the dielectric constant and volume resistivity; Combining the data of Example 1, Example 9 and Comparative Example 2, it can be seen that the flame retardant has almost no effect on the insulation performance of the composite material.

[0077] A scanning electron microscope image of a plastic particle used for processing electrical product housings, such as Figure 2 As shown, specifically, it is a scanning electron microscope image of Example 1 with the best comprehensive performance. The modified glass fiber forms multiple layers, and there are gaps between the glass fibers to form a porous structure for accommodating flame retardant molecules. The flame will be hindered when propagating in the material, making it difficult for heat to be quickly transferred to the entire material.

Claims

1. A plastic particle formula for processing electrical product housings, characterized in that: The formula is calculated by weight, and its raw materials include the following components: 60-90 parts of PA66, 10-40 parts of modified glass fiber, 0.1-0.6 parts of antioxidant, 0.2-1 parts of lubricant, 10-20 parts of flame retardant, and 2-5 parts of other additives.

2. The plastic particle formula for electrical product housing processing according to claim 1, characterized in that: Modified glass fibers include modified round-section glass fibers and modified flat glass fibers.

3. The plastic particle formula for electrical product housing processing according to claim 2, characterized in that: The modification method of the modified glass fiber is: A1. Weigh and mix the silane coupling agent, deionized water and anhydrous ethanol in a mass ratio of 1:30:30 to prepare a modified solution; A2, dissolving, adding the modified solution at a ratio of 10 ml per 1 g of glass fiber, stirring thoroughly for 10-20 minutes, and ultrasonicating for 1-2 hours; A3. Drying: Take out and dry in a constant temperature drying oven at 100 degrees Celsius for 6-8 hours to obtain the modified glass fiber.

4. The plastic particle formula for electrical product housing processing according to claim 3, characterized in that: The other additives include voltage stabilizers and silica sol.

5. The plastic particle formula for electrical product housing processing according to claim 4, characterized in that: The voltage stabilizer comprises a sterically hindered piperidine free radical scavenger and an organic substance containing an ortho-phenolic hydroxyl group and an ethylene oxide branch chain.

6. A process for preparing plastic particles for processing electrical product shells, using a plastic particle formula for processing electrical product shells as described in any one of claims 1 to 5, characterized in that: The following steps are involved: S1. PA66 is placed in a constant temperature drying oven and dried for 4-5 hours. The temperature of the constant temperature drying oven is set at 75-85 degrees Celsius. S2, take out the PA66 in the constant temperature drying oven, weigh the corresponding mass together with the other raw materials, add them into the twin-screw extruder according to the proportion, and perform heating and melting, plasticizing and mixing, extrusion granulation, cooling and solidification, separation and screening, and anti-static packaging and storage operations; S3, drying the obtained plastic particles in a constant temperature drying oven at 100 degrees Celsius for 5-6 hours, and forming standard specimens through an injection molding machine; S4. Take out the prepared standard sample and let it stand for 24 hours before measuring the material index.

7. The process for preparing plastic particles for electrical product housing processing according to claim 6, characterized in that: The process parameters of the twin-screw extruder are as follows: the temperature of zone 1 is 140-160 degrees Celsius, the temperature of zone 2 is 270-280 degrees Celsius, the temperature of zone 3 is 270-280 degrees Celsius; the temperature of zone 4 is 260-270 degrees Celsius; the temperature of zone 5 is 260-270 degrees Celsius; the temperature of zone 6 is 250-270 degrees Celsius; the temperature of zone 7 is 255-270 degrees Celsius; the temperature of zone 8 is 260-270 degrees Celsius; the temperature of zone 9 is 260-270 degrees Celsius; the head temperature is 265 degrees Celsius; the vacuum degree is 0.04-0.06 MPa; the main engine speed is 700-750 r / min; the feeding speed is 420-450 r / min; and the pelletizing speed is 400-650 r / min.

8. The process for preparing plastic particles for electrical product housing processing according to claim 6, characterized in that: The process parameters of the injection molding machine are: The temperature of zone 1 is 270 degrees Celsius; the temperature of zone 2 is 260 degrees Celsius; the temperature of zone 3 is 260 degrees Celsius; the temperature of zone 4 is 260 degrees Celsius; the temperature of zone 5 is 265 degrees Celsius; the injection pressure is 60-80 MPa; the injection speed is 35-45cm 3 / s, injection time is 26s.

Citation Information

Patent Citations

  • Flame-retardant glass-fiber-reinforced polyamide resin composition

    CN101796137A

  • Electrical and electronic equipment part formed by injection moulding of glass fibre reinforced resin composition

    CN101928451A

  • Thermally conductive insulating glass fiber reinforced flame-retardant PA66 and preparation method thereof

    CN109280378A

  • Composite plastic particles and preparation method thereof

    CN113845770A

  • High-voltage ultra-clean insulating material with excellent anti-aging performance and preparation method of high-voltage ultra-clean insulating material

    CN117070008A