Ultraviolet induction type allochroic silica gel pad and preparation method thereof

By using silica microspheres as support and catalyst for spiropyran dye in ultraviolet-sensitivity discoloration silicone pads, the problem of poor fatigue resistance of existing silicone pads is solved, its stability and service life are improved, and the application range is expanded .

CN119081410APending Publication Date: 2024-12-06FENGYANG JIASONG NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411369962.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing ultraviolet-sensing discolored silicone pads have poor fatigue resistance and are easily affected by factors such as oxygen, pH, light and temperature, resulting in oxidation, limiting its use range.

Method used

UV-induced color-changing silicone pad composed of polydimethylsiloxane, spiropyran dye, platinum catalyst, silica microspheres, calcium stearate, sodium gluconate, vulcanizing agent and crosslinking agent, through specific The process steps and material optimization include the preparation of silica microspheres and the treatment of spiropyran dyes to improve the fatigue stability of the silicone pad.

Benefits of technology

By using silica microspheres as support and catalyst for spiropyran dye, the fatigue resistance and service life of the silicone pad are improved, the application range is expanded, and the resistance to oxidation is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005067323920000101
    Figure BDA0005067323920000101
  • Figure BDA0005067323920000111
    Figure BDA0005067323920000111
Patent Text Reader

Abstract

The invention relates to an ultraviolet induction type allochroic silica gel pad and a preparation method thereof, and belongs to the technical field of silica gel products. The silicone rubber is prepared from the following raw materials: 80 to 120 parts of polydimethylsiloxane, 1 to 5 parts of spiropyrane dye, 0.01 to 0.05 part of platinum catalyst, 10 to 15 parts of silicon dioxide microspheres, 1.5 to 2 parts of calcium stearate, 1.5 to 2 parts of sodium gluconate, 1.5 to 2 parts of vulcanizing agent and 1 to 2 parts of cross-linking agent. The silica microspheres and the spiropyrane dye are combined, silicon hydroxyl residues on the surface of silica gel are eliminated through the silica microspheres, the compatibility of the spiropyrane dye and polydimethylsiloxane can be improved, the fatigue resistance stability of the allochroic silica gel is improved, and silica has excellent light permeability and insulativity, so that the color-changing silica gel is suitable for being used in the fields of photochromic materials and photochromic materials, and the service life of the color-changing silica gel is prolonged. The color change characteristic of the spiropyrane dye can be reflected to the maximum extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silica gel products, and in particular relates to an ultraviolet-sensitive color-changing silica gel pad and a preparation method thereof. Background Art

[0002] UV-sensitive color-changing silica gel will produce a color-changing effect after absorbing ultraviolet rays. It can be applied to clothing, environment, medical and other fields, and has certain economic benefits. The existing UV-sensitive color-changing silica gel is made by mixing the treated silica gel matrix with the UV-sensitive agent or color-changing material in a certain proportion, and then using certain process steps (such as dipping, stirring, standing, etc.) to evenly distribute the UV-sensitive agent or color-changing material on the pore surface inside the silica gel. Common UV-sensitive agents or color-changing materials include photosensitive OP powder, MC powder, spiropyran dyes, etc. However, although the above-mentioned UV-sensitive agents or color-changing materials have the unique property of photochromism, they have poor fatigue resistance and are easily affected by factors such as oxygen, pH value, light and temperature and oxidized. Even if antioxidants are added, the effect is not very obvious, which limits the scope of use of the color-changing silica gel pad. Summary of the invention

[0003] The purpose of the present invention is to provide a UV-sensitive color-changing silicone pad and a preparation method thereof in order to solve the above-mentioned problems.

[0004] The present invention achieves the above-mentioned purpose through the following technical solutions:

[0005] The invention provides an ultraviolet-sensitive color-changing silica gel pad, which is made of the following raw materials by weight: 80-120 parts of polydimethylsiloxane, 1-5 parts of spiropyran dye, 0.01-0.05 parts of platinum catalyst, 10-15 parts of silica microspheres, 1.5-2 parts of calcium stearate, 1.5-2 parts of sodium gluconate, 1.5-2 parts of vulcanizing agent, and 1-2 parts of cross-linking agent;

[0006] The preparation process of silica microspheres is as follows:

[0007] Mesoporous silica microspheres are dispersed in a sodium chloride solution at room temperature, stirred with ultrasound, filtered and vacuum dried, and then subjected to a two-stage heating treatment. In the first stage, the temperature is raised to 180-210°C and maintained for 0.5-1h, then raised to 450-500°C and maintained for 0.5-1h. After natural cooling, the temperature is washed several times with ethanol and deionized water to obtain silica microspheres.

[0008] As a further optimization scheme of the present invention, the pore size of the silica microspheres is 150-200 nm.

[0009] As a further optimization scheme of the present invention, the preparation process of the spiropyran dye is as follows: 50 g / L of the spiropyran photochromic dye is added to a Tween emulsifier aqueous solution, and after ultrasonic treatment for 0.5-1 h, the spiropyran dye is obtained.

[0010] As a further optimization scheme of the present invention, 50 g / L of spiropyran photochromic dye is added to a Tween emulsifier aqueous solution, stirred evenly, and then an antioxidant is added. After ultrasonic treatment for 0.5-1 h, the spiropyran dye is obtained.

[0011] As a further optimization scheme of the present invention, 50 g / L of spiropyran photochromic dye is added to the Tween emulsifier aqueous solution, and after stirring evenly, 10 g / L of ethylenediamine is added to the Tween emulsifier aqueous solution, and after ultrasonication for 0.5-1 h, the spiropyran dye is obtained.

[0012] As a further optimization scheme of the present invention, the Tween emulsifier aqueous solution is a Tween 80 emulsifier aqueous solution with a mass fraction of 5-10wt%.

[0013] As a further optimization scheme of the present invention, the vulcanizing agent is one of dipentadiene and tert-butyl perbenzoate.

[0014] As a further optimization scheme of the present invention, the cross-linking agent is a multifunctional polycarbodiimide cross-linking agent.

[0015] The present invention also provides a method for preparing the above-mentioned ultraviolet-sensitive color-changing silica gel pad, comprising the following steps:

[0016] (1) mixing silica microspheres and spiropyran dyes uniformly, adding a crosslinking agent dropwise to the mixture, adding a vulcanizing agent, calcium stearate, sodium gluconate and the mixture to polyorganosiloxane, stirring uniformly and standing at 40-50° C. for 0.5-1 h to obtain a silica gel material;

[0017] (2) adding the silica gel material to an open mill, starting the open mill and adjusting the roller speed ratio, then adding a coolant at 30-40° C. for mixing, and mixing for 10-15 min. After the mixed material is fully soft and the surface is smooth and flat, the material is discharged and a sheet is obtained;

[0018] (3) After the silicone pad is pressed out into a semi-finished product, it is continuously vulcanized by hot air to obtain a color-changing silicone pad.

[0019] As a further optimization scheme of the present invention, the vulcanization temperature is 180-220° C., and the vulcanization time is 5-8 min.

[0020] The beneficial effects of the present invention are:

[0021] (1) The present invention utilizes silica microspheres to eliminate the residual silanol groups on the surface of silica gel, which helps to improve the compatibility of spiropyran dyes with polydimethylsiloxane, increase the fatigue resistance stability of the color-changing silica gel, and increase the fatigue resistance stability of the silica gel pad.

[0022] (2) The present invention selects silica microspheres as the carrier of spiropyran dyes. Compared with the traditional spiropyran dye microcapsule technology, the process steps are simple, and the silica microspheres can also be used as a catalyst or auxiliary agent to increase the cross-linking reaction rate. At the same time, they can be used as a preservative to effectively prevent silica gel corrosion and increase the service life of silica gel. DETAILED DESCRIPTION

[0023] The present application is described in further detail below. It is necessary to point out that the following specific implementation methods are only used to further illustrate the present application and cannot be understood as limiting the scope of protection of the present application. Technicians in this field can make some non-essential improvements and adjustments to the present application based on the above application content.

[0024] 1. Materials

[0025] Unless otherwise specified, the methods used in the present invention are conventional methods known to those skilled in the art, and the reagents and other materials used are commercially available products unless otherwise specified.

[0026] The spiropyran dyes of the present invention include but are not limited to N, N′-1, 4-butylene bispiropyran, indoline benzospiropyran, and N-octyl-3, 3-dimethylindoline-6′-nitrobenzospiropyran. The spiropyran dyes in the following examples are purchased from Xi'an Qiyue Biotechnology Co., Ltd., specifically N-octyl-3, 3-dimethylindoline-6′-nitrobenzospiropyran.

[0027] The vulcanizing agent of the present invention is one of di-2-pentane and tert-butyl perbenzoate. The vulcanizing agent in the following embodiments is di-2-pentane.

[0028] The crosslinking agent of the present invention is a multifunctional polycarbodiimide (EDAC) crosslinking agent purchased from Xi'an Qiyue Biotechnology Co., Ltd.

[0029] The platinum catalyst of the present invention is purchased from Anhui Aiyota Silicone Oil Co., Ltd.

[0030] 2. Methods

[0031] Example 1

[0032] The present embodiment provides a UV-sensitive color-changing silicone pad, which is made of the following raw materials by weight: 100 parts of polydimethylsiloxane, 2 parts of spiropyran dye, 0.01 parts of platinum catalyst, 10 parts of silica microspheres, 1.5 parts of calcium stearate, 1.5 parts of sodium gluconate, 1.5 parts of vulcanizing agent, and 2 parts of cross-linking agent;

[0033] in:

[0034] Preparation of silica microspheres: 1 kg of mesoporous silica microspheres (10-50 nm) were dispersed into 10 L of 5% sodium chloride solution at room temperature, stirred for 3 h and ultrasonicated, filtered and vacuum dried for 2 h, and then transferred to a high-temperature box furnace for a two-stage heating treatment. In the first stage, the temperature was uniformly raised to 200°C and maintained for 1 h, then uniformly raised to 500°C and maintained for 0.5 h. After naturally cooling to room temperature, the temperature was washed 3 times with ethanol and deionized water, and dried to obtain silica microspheres. The pore size range of the silica microspheres was 150-200 nm.

[0035] Preparation of spiropyran dye: 50 g / L of spiropyran photochromic dye was added to a 5 wt % Tween 80 emulsifier aqueous solution, and the spiropyran dye was obtained after ultrasonic treatment for 0.5 h.

[0036] The preparation method of the color-changing silica gel pad is as follows:

[0037] (1) First, the silica microspheres and the spiropyran dye are mixed evenly, and the crosslinking agent is added dropwise to the mixture at a rate of 60 drops / min, with each drop being no less than 2 ml;

[0038] (2) adding a vulcanizing agent, calcium stearate, sodium gluconate and the mixed solution to the polyorganosiloxane, stirring the mixture evenly and standing it at 50° C. for 0.5 h to obtain a silica gel material;

[0039] (3) Add the silica gel material to the open mill, start the open mill and adjust the roller speed ratio to 1:1.2, then add a 30°C coolant for mixing, and the mixing time is 15 minutes. After the mixed material is fully soft and the surface is smooth and flat, the material is discharged to obtain a silica gel pad;

[0040] (4) The above-mentioned silicone pad is pressed into a semi-finished product through a mold and then continuously vulcanized with hot air at 190° C. for 8 minutes to obtain a color-changing silicone pad.

[0041] Example 2

[0042] The present embodiment provides a UV-sensitive color-changing silicone pad, which is made of the following raw materials by weight: 120 parts of polydimethylsiloxane, 5 parts of spiropyran dye, 0.01 parts of platinum catalyst, 15 parts of silica microspheres, 2 parts of calcium stearate, 2 parts of sodium gluconate, 1.5 parts of vulcanizing agent, and 2 parts of cross-linking agent;

[0043] in:

[0044] Preparation of silica microspheres: 1 kg of mesoporous silica microspheres (10-50 nm) were dispersed into 10 L of 5% sodium chloride solution at room temperature, stirred for 3 h and ultrasonicated, filtered and vacuum dried for 2 h, and then transferred to a high-temperature box furnace for a two-stage heating treatment. In the first stage, the temperature was uniformly raised to 200°C and maintained for 1 h, then uniformly raised to 500°C and maintained for 0.5 h. After naturally cooling to room temperature, the temperature was washed three times with ethanol and deionized water, and dried to obtain silica microspheres. The pore size range of the silica microspheres was 150-200 nm.

[0045] Preparation of spiropyran dye: 50 g / L of spiropyran photochromic dye was added to 5 wt% Tween 80 emulsifier aqueous solution, stirred evenly, and then 10 g / L of antioxidant 168 was added to the Tween 80 emulsifier aqueous solution. After ultrasonic treatment for 0.5 h, the spiropyran dye was obtained.

[0046] The preparation method of the color-changing silica gel pad is as follows:

[0047] (1) First, the silica microspheres and the spiropyran dye are mixed evenly, and the crosslinking agent is added dropwise to the mixture at a rate of 60 drops / min, with each drop being no less than 2 ml;

[0048] (2) adding a vulcanizing agent, calcium stearate, sodium gluconate and the mixed solution to the polyorganosiloxane, stirring the mixture evenly and standing it at 50° C. for 0.5 h to obtain a silica gel material;

[0049] (3) Add the silica gel material to the open mill, start the open mill and adjust the roller speed ratio to 1:1.2, then add a 30°C coolant for mixing, and the mixing time is 15 minutes. After the mixed material is fully soft and the surface is smooth and flat, the material is discharged to obtain a silica gel pad;

[0050] (4) The above-mentioned silicone pad is pressed into a semi-finished product through a mold and then continuously vulcanized with hot air at 190° C. for 8 minutes to obtain a color-changing silicone pad.

[0051] Example 3

[0052] The present embodiment provides a UV-sensitive color-changing silicone pad, which is made of the following raw materials by weight: 120 parts of polydimethylsiloxane, 5 parts of spiropyran dye, 0.01 parts of platinum catalyst, 15 parts of silica microspheres, 2 parts of calcium stearate, 2 parts of sodium gluconate, 1.5 parts of vulcanizing agent, and 2 parts of cross-linking agent;

[0053] in:

[0054] Preparation of silica microspheres: 1 kg of mesoporous silica microspheres (10-50 nm) were dispersed into 10 L of 5% sodium chloride solution at room temperature, stirred for 3 h and ultrasonicated, filtered and vacuum dried for 2 h, and then transferred to a high-temperature box furnace for a two-stage heating treatment. In the first stage, the temperature was uniformly raised to 200°C and maintained for 1 h, then uniformly raised to 500°C and maintained for 0.5 h. After naturally cooling to room temperature, the temperature was washed 3 times with ethanol and deionized water, and dried to obtain silica microspheres. The pore size range of the silica microspheres was 150-200 nm.

[0055] Preparation of spiropyran dye: 50 g / L of spiropyran photochromic dye was added to a 5 wt% Tween 80 emulsifier aqueous solution, stirred evenly, and then 10 g / L of ethylenediamine was added to the Tween emulsifier aqueous solution. After ultrasonic treatment for 0.5 h, the spiropyran dye was obtained.

[0056] The preparation method of the color-changing silica gel pad is as follows:

[0057] (1) First, the silica microspheres and the spiropyran dye are mixed evenly, and the crosslinking agent is added dropwise to the mixture at a rate of 60 drops / min, with each drop being no less than 2 ml;

[0058] (2) adding a vulcanizing agent, calcium stearate, sodium gluconate and the mixed solution to the polyorganosiloxane, stirring the mixture evenly and standing it at 50° C. for 0.5 h to obtain a silica gel material;

[0059] (3) Add the silica gel material to the open mill, start the open mill and adjust the roller speed ratio to 1:1.2, then add a 30°C coolant for mixing, and the mixing time is 15 minutes. After the mixed material is fully soft and the surface is smooth and flat, the material is discharged to obtain a silica gel pad;

[0060] (4) The above-mentioned silicone pad is pressed into a semi-finished product through a mold and then continuously vulcanized with hot air at 190° C. for 8 minutes to obtain a color-changing silicone pad.

[0061] Comparative Example 1

[0062] The silica gel pad is made of the following raw materials by weight: 120 parts of polydimethylsiloxane, 5 parts of spiropyran dye, 0.01 parts of platinum catalyst, 15 parts of silica microspheres, 2 parts of calcium stearate, 2 parts of sodium gluconate, 1.5 parts of vulcanizing agent, and 2 parts of cross-linking agent;

[0063] The preparation of spiropyran dye: using N-octyl-3,3-dimethylindoline-6'-nitrobenzospiropyran as core material, polymethyl methacrylate and ethyl cellulose as wall materials, preparing spiropyran dye microcapsules by solvent evaporation method as spiropyran dye.

[0064] The remaining raw materials and preparation method are the same as in Example 3.

[0065] Comparative Example 2

[0066] The silica gel pad is made of the following raw materials by weight: 120 parts of polydimethylsiloxane, 5 parts of spiropyran dye, 0.01 parts of platinum catalyst, 15 parts of silica microspheres, 2 parts of calcium stearate, 2 parts of sodium gluconate, 1.5 parts of vulcanizing agent, and 2 parts of cross-linking agent;

[0067] Among them, the silica microspheres directly use mesoporous silica microspheres with a pore size range of 10-50nm.

[0068] The remaining raw materials and preparation method are the same as in Example 3.

[0069] Comparative Example 3

[0070] The silica gel pad is made of the following raw materials by weight: 120 parts of polydimethylsiloxane, 5 parts of spiropyran dye, 0.01 parts of platinum catalyst, 15 parts of silica microspheres, 2 parts of calcium stearate, 2 parts of sodium gluconate, 1.5 parts of vulcanizing agent, and 2 parts of cross-linking agent;

[0071] The silica microspheres are directly commercially available macroporous silica microspheres with a pore size range of 300-500 nm.

[0072] The remaining raw materials and preparation method are the same as in Example 3.

[0073] Comparative Example 4

[0074] The silica gel pad is made of the following raw materials by weight: 120 parts of polydimethylsiloxane, 5 parts of spiropyran dye, 0.05 parts of platinum catalyst, 15 parts of fumed silica, 2 parts of calcium stearate, 2 parts of sodium gluconate, 1.5 parts of vulcanizing agent, and 2 parts of cross-linking agent;

[0075] The preparation method of the color-changing silica gel pad is as follows:

[0076] (1) First, fumed silica and spiropyran dye are mixed evenly, and a crosslinking agent is added dropwise to the mixture at a rate of 60 drops / min, with each drop being no less than 2 ml;

[0077] (2) adding a vulcanizing agent, calcium stearate, sodium gluconate and the mixed solution to the polyorganosiloxane, stirring the mixture evenly and standing it at 50° C. for 2 hours to obtain a silica gel material;

[0078] (3) Add the silica gel material to the open mill, start the open mill and adjust the roller speed ratio to 1:1.2, then add 30°C coolant for mixing, and the mixing time is 60 minutes. After the mixed material is fully soft and the surface is smooth and flat, the material is discharged to obtain a silica gel pad;

[0079] (4) The above-mentioned silicone pad is pressed into a semi-finished product through a mold and then continuously vulcanized with hot air at 220° C. for 8 minutes to obtain a color-changing silicone pad.

[0080] Comparative Example 5

[0081] The silica gel pad has the same raw material components as in Example 3, and its preparation method is as follows:

[0082] (1) adding silica microspheres, spiropyran dye, vulcanizing agent, crosslinking agent, calcium stearate and sodium gluconate to polyorganosiloxane, stirring evenly and standing at 50° C. for 0.5 h to obtain silica gel;

[0083] (2) Add the silica gel material into the open mill, start the open mill and adjust the roller speed ratio to 1:1.2, then add 30°C coolant for mixing, and the mixing time is 20 minutes. After the mixed material is fully soft and the surface is smooth and flat, the material is discharged to obtain a silica gel pad;

[0084] (3) The above-mentioned silicone pad is pressed into a semi-finished product through a mold and then continuously vulcanized with hot air at 190° C. for 8 minutes to obtain a color-changing silicone pad.

[0085] 3. Test Verification

[0086] Using the color-changing silica gel pads prepared in Examples 1-3 and Comparative Examples 1-5, cut samples of appropriate size as test samples and conduct the following tests:

[0087] Tear strength: The tear strength of each sample was measured using a WDS series universal testing machine, and the average value was taken after 5 measurements.

[0088] Fatigue resistance: The test samples were tested with a colorimeter. During the test, the initial chromaticity of the samples was measured under a xenon arc lamp simulating ultraviolet light (GB / T16422.2 Plastics Laboratory Light Source Exposure Test Method Part 2 Xenon Arc Lamp), which was recorded as S1. Then, the samples were placed in a UV aging box for 48 hours. After cooling and standing, the samples were placed in the same xenon arc lamp simulating ultraviolet light environment, and the chromaticity of the silicone pad was measured, which was recorded as S2. The decolorization rate was (S1-S2) / S1×100%.

[0089] The YH1200 haze meter was used to measure the light transmittance of each sample after it was placed in a UV aging box for 48 hours, and the average value was taken after 5 measurements.

[0090] The test results are recorded in the following table:

[0091]

[0092]

[0093] It can be seen from Examples 1-3 and Comparative Example 1 that the present invention selects silica microspheres as the support of spiropyran dyes. Compared with the traditional spiropyran dye microcapsule technology, the process steps are simple, and the silica microspheres can also be used as a catalyst or auxiliary agent to increase the crosslinking reaction rate, and can also be used as a preservative to effectively prevent silica gel corrosion and increase the service life of silica gel. Compared with the traditional reinforcing agent fumed silica (Comparative Example 4), adding silica microspheres to polydimethylsiloxane will have a slight effect on the tear strength, but increase the fatigue resistance.

[0094] It can be seen from Examples 1-3 and Comparative Examples 2-3 that, compared with mesoporous silica microspheres and macroporous silica microspheres, the present invention utilizes treated silica microspheres to eliminate residual silanol groups on the surface of silica gel, which helps to improve the compatibility of spiropyran dyes with polydimethylsiloxane and further increase the fatigue resistance stability of the color-changing silica gel.

[0095] It can be seen from Examples 1-3 and Comparative Example 5 that during the preparation of the present invention, the silica microspheres and the spiropyran dye are first mixed evenly, and the cross-linking agent is added dropwise to the mixture, so that the spiropyran dye can be locked in the silica microspheres, reducing the degree of oxidation caused by factors such as oxygen, pH value, light and temperature, thereby expanding the scope of use of the color-changing silica gel pad.

[0096] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A UV-sensitive color-changing silicone pad, characterized in that: The raw materials are as follows: 80-120 parts of polydimethylsiloxane, 1-5 parts of spiropyran dye, 0.01-0.05 parts of platinum catalyst, 10-15 parts of silica microspheres, 1.5-2 parts of calcium stearate, 1.5-2 parts of sodium gluconate, 1.5-2 parts of vulcanizing agent, and 1-2 parts of cross-linking agent. The preparation process of silica microspheres is as follows: Mesoporous silica microspheres are dispersed in a sodium chloride solution at room temperature, stirred with ultrasound, filtered and vacuum dried, and then subjected to a two-stage heating treatment. In the first stage, the temperature is raised to 180-210°C and maintained for 0.5-1h, then raised to 450-500°C and maintained for 0.5-1h. After natural cooling, the temperature is washed several times with ethanol and deionized water to obtain silica microspheres.

2. The ultraviolet-sensitive color-changing silicone pad according to claim 1, characterized in that: The pore size of the silica microspheres is 150-200 nm.

3. The ultraviolet-sensitive color-changing silicone pad according to claim 1, characterized in that: The preparation process of the spiropyran dye is as follows: 50 g / L of the spiropyran photochromic dye is added into a Tween emulsifier aqueous solution, and the spiropyran dye is obtained after ultrasonic treatment for 0.5-1 h.

4. The ultraviolet-sensitive color-changing silicone pad according to claim 3, characterized in that: The spiropyran photochromic dye is added into the Tween emulsifier aqueous solution at 50 g / L, stirred evenly, and then an antioxidant is added. After ultrasonic treatment for 0.5-1 h, the spiropyran dye is obtained.

5. The ultraviolet-sensitive color-changing silicone pad according to claim 3, characterized in that: 50 g / L of spiropyran photochromic dye was added to a Tween emulsifier aqueous solution, and after being stirred evenly, 10 g / L of ethylenediamine was added to the Tween emulsifier aqueous solution, and after ultrasonic treatment for 0.5-1 h, a spiropyran dye was obtained.

6. A UV-sensitive color-changing silicone pad according to any one of claims 3 to 5, characterized in that: The Tween emulsifier aqueous solution is a Tween 80 emulsifier aqueous solution with a mass fraction of 5-10wt%.

7. The ultraviolet-sensitive color-changing silicone pad according to claim 1, characterized in that: The vulcanizing agent is one of dipentadienyl and tert-butyl perbenzoate.

8. The ultraviolet-sensitive color-changing silicone pad according to claim 1, characterized in that: The cross-linking agent is a multifunctional polycarbodiimide cross-linking agent.

9. A method for preparing the ultraviolet-sensitive color-changing silicone pad as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: (1) mixing silica microspheres and spiropyran dyes uniformly, adding a crosslinking agent dropwise to the mixture, adding a vulcanizing agent, calcium stearate, sodium gluconate and the mixture to polyorganosiloxane, stirring uniformly and standing at 40-50° C. for 0.5-1 h to obtain a silica gel material; (2) adding the silica gel material to an open mill, starting the open mill and adjusting the roller speed ratio, then adding a coolant at 30-40° C. for mixing, and mixing for 10-15 min. After the mixed material is fully soft and the surface is smooth and flat, the material is discharged and a sheet is obtained; (3) After the silicone pad is pressed out into a semi-finished product, it is continuously vulcanized by hot air to obtain a color-changing silicone pad.

10. The method for preparing a UV-sensitive color-changing silicone pad according to claim 9, characterized in that: The vulcanization temperature is 180-220° C., and the vulcanization time is 5-8 minutes.