High-temperature-resistant and wear-resistant composite asphalt material as well as preparation method and application thereof

By using the combination of lake asphalt, lignin sulfonic acid rinsic modified asphalt, waste ceramic particles and oyster shell modified rubber particles, the wear resistance and high temperature stability of the asphalt pavement are improved, and the resistance of the asphalt pavement in the existing technology Zhonghu asphalt pavement is solved The problem of poor wearability achieves a longer service life and a more economical and environmentally friendly solution.

CN119081433APending Publication Date: 2024-12-06GUOGAO TRANSPORTATION TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411494011.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, the asphalt pavement with lake asphalt as the main raw material has poor wear resistance and insufficient high-temperature stability, resulting in easy softening and damage in a high-temperature environment.

Method used

The high temperature stability and rut resistance of composite asphalt materials are used as raw materials, and the high temperature stability and rut resistance of composite asphalt materials are improved by forming a three-dimensional network structure and synergistic effect. Relieve treatment pressure through the utilization of waste ceramics and waste rubber.

Benefits of technology

It significantly improves the wear resistance and mechanical properties of composite asphalt materials, extends the service life, simplifies the preparation process, and provides economical and environmentally friendly technical solutions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of highway pavement materials, in particular to a high-temperature-resistant and wear-resistant composite asphalt material as well as a preparation method and application thereof. The high-temperature-resistant and wear-resistant composite asphalt material comprises the following raw material components in percentage by mass: 25-80% of lake asphalt, 3-6% of lignosulfonate modified asphalt, 5-8% of waste ceramic particles and the balance of oyster shell modified rubber particles. The high-temperature-resistant and wear-resistant composite asphalt material is simple in component, simple and convenient in preparation process and excellent in performance, effectively solves the problems of poor wear resistance and limited service life of an asphalt pavement taking lake asphalt as a main raw material in the prior art, and provides a more economical and environment-friendly technical scheme for a highway pavement material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of highway pavement materials, and in particular to a high-temperature-resistant and wear-resistant composite asphalt material and a preparation method and application thereof. Background Art

[0002] Asphalt pavement accounts for a large proportion of modern high-grade highways due to its advantages such as low driving noise, good comfort, no dust, and relatively simple maintenance. According to statistics, about 90% of the high-grade highways that have been built use asphalt concrete pavement. However, with the formation of the expressway network and the rapid development of the national economy, the road traffic volume is increasing day by day, and the proportion of overloaded vehicles is increasing rapidly. The looseness, potholes, cracks and rutting of asphalt pavement are becoming more and more serious. Based on this, engineers have proposed a variety of solutions.

[0003] Lake asphalt (TLA asphalt) is a naturally formed asphalt. When mixed with petroleum asphalt, it can effectively improve the road performance of petroleum asphalt, such as high temperature stability and resistance to water damage. Lake asphalt modified asphalt pavement has been widely praised by users for its strong environmental adaptability, ultra-long service life, and low maintenance costs.

[0004] However, it has been found through actual use that although the addition of lake asphalt can improve the road performance of asphalt pavement to a certain extent, due to the large amount of water contained in lake asphalt, the wear resistance of asphalt pavement is poor, and its softening point is easily reduced under high temperature environment. Therefore, the development of an asphalt material containing lake asphalt and having high wear resistance and high temperature stability is of great significance to the development of highway pavement materials. Summary of the invention

[0005] In view of the problem that the asphalt pavement with lake asphalt as the main raw material in the prior art has poor wear resistance and poor high temperature stability, the present invention provides a high temperature wear-resistant composite asphalt material and its preparation method and application. The present invention uses lake asphalt, lignin sulfonate modified asphalt, waste ceramic particles and oyster shell modified rubber particles as raw materials to prepare a high temperature wear-resistant composite asphalt material with wear resistance and excellent mechanical properties. The high temperature wear-resistant composite asphalt material has simple ingredients and a simple preparation process, and uses waste ceramics and waste rubber as raw materials, which greatly alleviates the processing pressure of these two wastes and provides a more economical and environmentally friendly technical solution for highway pavement materials.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions: The first aspect of the present invention provides a high temperature resistant and wear resistant composite asphalt material, comprising the following raw material components in percentage by weight: 25%-80% lake asphalt, 3%-6% lignin sulfonate modified asphalt, 5%-8% waste ceramic particles and the remainder oyster shell modified rubber particles.

[0007] Compared with the prior art, the present invention uses lake asphalt and lignin sulfonate modified asphalt as the main components, and utilizes the high asphaltene characteristics and gel structure of lake asphalt to effectively improve the high temperature stability and softening point of composite asphalt materials and the anti-rutting ability of composite asphalt materials. In addition, the high nitrogen content of lake asphalt can increase the viscosity and oxidation resistance of composite asphalt materials, further improving the durability of composite asphalt materials, so that they can still maintain stable performance at higher temperatures and have a longer service life. The cross-linking effect between lignin and asphalt molecules in lignin sulfonate modified asphalt will form a three-dimensional network structure, in which waste ceramic particles and oyster shell modified rubber particles can be filled, comprehensively improving the mechanical properties of composite asphalt materials.

[0008] At the same time, a synergistic effect can be formed between lake asphalt and lignin sulfonate modified asphalt, and the waste ceramic particles and oyster shell modified rubber particles coated therein are used to absorb and capture the moisture in the lake asphalt, thereby alleviating the problem that the lake asphalt has poor wear resistance due to its high moisture content. In order to further enhance the wear resistance of the composite asphalt material, the present invention also modifies the rubber particles. Oyster shells contain a large amount of calcium carbonate and a small amount of organic and inorganic trace elements. The rich calcium source combines with the organic molecules in the rubber to easily form hydroxyapatite derivatives, which can improve the surface roughness of the material. The high temperature wear-resistant composite asphalt material of the present invention not only has excellent mechanical properties, but also has high wear resistance and high temperature stability, which effectively solves the problem of poor wear resistance and poor high temperature stability of asphalt pavement with lake asphalt as the main raw material in the prior art. More importantly, the high temperature wear-resistant composite asphalt material has simple ingredients, simple preparation process, and uses waste ceramics and waste rubber as raw materials, which greatly alleviates the processing pressure of these two wastes, and provides a more economical and environmentally friendly technical solution for highway pavement materials.

[0009] Preferably, the method for preparing the oyster shell modified rubber particles comprises the following steps: S1, ball-milling the oyster shells, heating to 300-350° C., and keeping the temperature, to obtain pretreated oyster shell powder; S2, crushing the waste rubber, mixing it once at 120-160° C., adding an anti-aging agent and the pretreated oyster shell powder, heating it to 170-180° C. for secondary mixing to obtain a rubber compound; S3, adding an accelerator and a vulcanizing agent to the rubber mixture for vulcanization, cooling, and granulating to obtain oyster shell modified rubber particles.

[0010] Further preferably, in S1, the rotation speed of the ball mill is 600-800 rpm, and the time of the ball mill is 30-50 min.

[0011] Further preferably, in S1, the temperature is raised to 300-350°C by programmed heating, and the heating rate is 10-15°C / min.

[0012] Further preferably, in S1, the insulation time is 1-2h.

[0013] More preferably, in S2, the time of the first mixing is 5-8 min.

[0014] More preferably, in S2, the secondary mixing time is 3-5 min.

[0015] Further preferably, in S2, the amount of the anti-aging agent added is 3%-5% of the mass of the waste rubber.

[0016] Further preferably, in S2, the mass ratio of the pretreated oyster shell powder to the waste rubber is 0.3:1-0.5:1.

[0017] Further preferably, in S3, the amount of the accelerator added is 1%-3% of the mass of the rubber compound.

[0018] Further preferably, in S3, the amount of the vulcanizing agent added is 1%-3% of the mass of the rubber compound.

[0019] Preferably, the particle size of the waste ceramic particles is 50-100 μm.

[0020] Preferably, the particle size of the oyster shell modified rubber particles is 100-200 μm.

[0021] Preferably, the preparation method of the lignin modified asphalt comprises the following steps: Step a, heating the lignin sulfonate modified asphalt to 130-160° C. to obtain a fluid asphalt component; Step b: adding lignin sulfonate to the mobile asphalt component, heating to 150-180° C., and stirring to obtain lignin modified asphalt.

[0022] Further preferably, in step b, the amount of lignin sulfonate added is 5%-8% of the mass of the mobile asphalt component.

[0023] Further preferably, in step b, the rotation speed of the stirring treatment is 800-1000 rpm, and the time of the stirring treatment is 15-20 min.

[0024] Preferably, the raw material components include the following mass percentages: 35%-75% lake asphalt, 4%-5% lignin sulfonate modified asphalt, 6%-7% waste ceramic particles and the remainder oyster shell modified rubber particles.

[0025] The second aspect of the present invention provides a method for preparing the high temperature resistant and wear resistant composite asphalt material, comprising the following steps: Step 1: weigh lignin sulfonate modified asphalt according to the designed ratio, melt it at 120-140° C. to obtain a first asphalt component; weigh lake asphalt according to the designed ratio, melt it at 165-190° C. to obtain a second asphalt component; mix the first asphalt component and the second asphalt component evenly to obtain an asphalt component; Step 2: Keep the asphalt component at 170-185° C., add waste ceramic particles and oyster shell modified rubber particles according to the designed ratio, mix them evenly, and obtain a high temperature resistant and wear resistant composite asphalt material.

[0026] Preferably, in step 2, the insulation time is 30-50 minutes.

[0027] The third aspect of the present invention provides the use of the high temperature resistant and wear resistant composite asphalt material or the high temperature resistant and wear resistant composite asphalt material prepared by the preparation method of the high temperature resistant and wear resistant composite asphalt material in the development of highway pavement materials.

[0028] In summary, the present invention uses lake asphalt and lignin sulfonate modified asphalt as main components, supplemented by waste ceramic particles and oyster shell modified rubber particles, to prepare a composite asphalt material with high wear resistance and long service life. The high temperature and wear resistant composite asphalt material has simple ingredients, simple preparation process and excellent performance, which effectively solves the problem of poor wear resistance and limited service life of asphalt pavement with lake asphalt as main raw material in the prior art, and provides a more economical and environmentally friendly technical solution for highway pavement materials. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1 This embodiment provides a high temperature resistant and wear resistant composite asphalt material, which specifically includes the following contents: The high temperature resistant and wear resistant composite asphalt material comprises the following raw material components in percentage by weight: 75% lake asphalt, 5% lignin sulfonate modified asphalt, 6% waste ceramic particles and 14% oyster shell modified rubber particles.

[0031] The preparation method of the high temperature resistant and wear resistant composite asphalt material comprises the following steps: Step 1: weigh lignin sulfonate modified asphalt according to the designed ratio, melt it at 130° C. to obtain a first asphalt component; weigh lake asphalt according to the designed ratio, melt it at 180° C. to obtain a second asphalt component; mix the first asphalt component and the second asphalt component evenly to obtain an asphalt component; Step 2: Keep the asphalt component at 175° C. for 40 minutes, add waste ceramic particles and oyster shell modified rubber particles according to the designed ratio, mix well, and obtain a high temperature resistant and wear resistant composite asphalt material.

[0032] The method for preparing the oyster shell modified rubber particles comprises the following steps: S1, ball milling 50 g of oyster shell at a speed of 700 rpm for 40 min, heating to 320° C., and keeping the temperature for 1.5 h to obtain pretreated oyster shell powder; S2, crushing 150g of waste rubber, mixing once at 150°C for 6min, adding 4.5g of anti-aging agent SP and the pretreated oyster shell powder, heating to 175°C for secondary mixing for 4min, and obtaining a rubber compound; S3. Add 3 g of accelerator NS and 3 g of sulfur to the rubber mixture for vulcanization, cooling, and granulation to obtain oyster shell modified rubber particles with a particle size of 150 μm.

[0033] The preparation method of the lignin sulfonate modified asphalt comprises the following steps: Step a, heating the lignin sulfonate modified asphalt to 150° C. to obtain a fluid asphalt component; Step b: add 6% lignin sulfonate to the mobile asphalt component, heat to 170° C., and stir at a speed of 900 rpm for 18 minutes to obtain lignin sulfonate modified asphalt.

[0034] The particle size of the waste ceramic particles is 80 μm.

[0035] Example 2 This embodiment provides a high temperature resistant and wear resistant composite asphalt material, which specifically includes the following contents: The high temperature and wear resistant composite asphalt material comprises the following raw material components in percentage by mass: 80% lake asphalt, 5% lignin sulfonate modified asphalt, 6% waste ceramic particles and 9% oyster shell modified rubber particles.

[0036] The preparation method of the high temperature resistant and wear resistant composite asphalt material comprises the following steps: Step 1: weigh lignin sulfonate modified asphalt according to the designed ratio, melt it at 135° C. to obtain a first asphalt component; weigh lake asphalt according to the designed ratio, melt it at 180° C. to obtain a second asphalt component; mix the first asphalt component and the second asphalt component evenly to obtain an asphalt component; Step 2: Keep the asphalt component at 175° C. for 35 minutes, add waste ceramic particles and oyster shell modified rubber particles according to the designed ratio, mix well, and obtain a high temperature resistant and wear resistant composite asphalt material.

[0037] The method for preparing the oyster shell modified rubber particles comprises the following steps: S1, ball milling 50 g of oyster shell at a speed of 650 rpm for 40 min, heating to 325° C., and keeping the temperature for 1.5 h to obtain pretreated oyster shell powder; S2, crushing 150g of waste rubber, mixing once at 150°C for 6min, adding 4.5g of anti-aging agent SP and the pretreated oyster shell powder, heating to 175°C for secondary mixing for 4min, and obtaining a rubber compound; S3. Add 3 g of accelerator NS and 3 g of sulfur to the rubber mixture for vulcanization, cooling, and granulation to obtain oyster shell modified rubber particles with a particle size of 140 μm.

[0038] The preparation method of the lignin sulfonate modified asphalt comprises the following steps: Step a, heating the lignin sulfonate modified asphalt to 150° C. to obtain a fluid asphalt component; Step b: add 6% lignin sulfonate to the mobile asphalt component, heat to 170° C., and stir at a speed of 900 rpm for 18 minutes to obtain lignin sulfonate modified asphalt.

[0039] The particle size of the waste ceramic particles is 100 μm.

[0040] Example 3 This embodiment provides a high temperature resistant and wear resistant composite asphalt material, which specifically includes the following contents: The high temperature resistant and wear resistant composite asphalt material comprises the following raw material components in percentage by weight: 70% lake asphalt, 7% lignin sulfonate modified asphalt, 7% waste ceramic particles and 16% oyster shell modified rubber particles.

[0041] The preparation method of the high temperature resistant and wear resistant composite asphalt material comprises the following steps: Step 1: weigh lignin sulfonate modified asphalt according to the designed ratio, melt it at 130° C. to obtain a first asphalt component; weigh lake asphalt according to the designed ratio, melt it at 180° C. to obtain a second asphalt component; mix the first asphalt component and the second asphalt component evenly to obtain an asphalt component; Step 2: Keep the asphalt component at 175° C. for 45 minutes, add waste ceramic particles and oyster shell modified rubber particles according to the designed ratio, mix well, and obtain a high temperature resistant and wear resistant composite asphalt material.

[0042] The method for preparing the oyster shell modified rubber particles comprises the following steps: S1, ball milling 50 g of oyster shell at a speed of 680 rpm for 40 min, heating to 320° C., and keeping the temperature for 1.5 h to obtain pretreated oyster shell powder; S2, 150g of waste rubber was crushed, mixed at 150°C for 6min, 4.5g of antioxidant SP and the pretreated oyster shell powder were added, and the temperature was raised to 175°C for secondary mixing for 5min to obtain a rubber compound; S3. Add 3 g of accelerator NS and 3 g of sulfur to the rubber mixture for vulcanization, cooling, and granulation to obtain oyster shell modified rubber particles with a particle size of 150 μm.

[0043] The preparation method of the lignin sulfonate modified asphalt comprises the following steps: Step a, heating the lignin sulfonate modified asphalt to 150° C. to obtain a fluid asphalt component; Step b: add 6% lignin sulfonate to the mobile asphalt component, heat to 170° C., and stir at a speed of 900 rpm for 18 minutes to obtain lignin sulfonate modified asphalt.

[0044] The particle size of the waste ceramic particles is 90 μm.

[0045] Comparative Example 1 This comparative example provides a high temperature resistant and wear resistant composite asphalt material, which is different from Example 1 in that the oyster shell modified rubber particles in the high temperature resistant and wear resistant composite asphalt material are replaced with an equal amount of rubber particles, specifically including the following contents: The high temperature resistant and wear resistant composite asphalt material comprises the following raw material components in percentage by weight: 75% lake asphalt, 5% lignin sulfonate modified asphalt, 6% waste ceramic particles and 14% oyster shell modified rubber particles.

[0046] The preparation method of the high temperature resistant and wear resistant composite asphalt material comprises the following steps: Step 1: weigh lignin sulfonate modified asphalt according to the designed ratio, melt it at 130° C. to obtain a first asphalt component; weigh lake asphalt according to the designed ratio, melt it at 180° C. to obtain a second asphalt component; mix the first asphalt component and the second asphalt component evenly to obtain an asphalt component; Step 2: Keep the asphalt component at 175° C. for 40 minutes, add waste ceramic particles and rubber particles according to the designed ratio, mix them evenly, and obtain a high temperature resistant and wear resistant composite asphalt material.

[0047] The preparation method of the rubber particles comprises the following steps: crushing 150g of waste rubber, mixing it once at 150°C for 6min, adding 4.5g of anti-aging agent SP and heating it to 175°C for secondary mixing for 4min to obtain a rubber mixture; adding 3g of accelerator NS and 3g of sulfur to the rubber mixture for vulcanization, cooling, and granulating to obtain rubber particles with a particle size of 150μm.

[0048] The preparation method of the lignin sulfonate modified asphalt comprises the following steps: Step a, heating the lignin sulfonate modified asphalt to 150° C. to obtain a fluid asphalt component; Step b: add 6% lignin sulfonate to the mobile asphalt component, heat to 170° C., and stir at a speed of 900 rpm for 18 minutes to obtain lignin sulfonate modified asphalt.

[0049] The particle size of the waste ceramic particles is 80 μm.

[0050] Comparative Example 2 This comparative example provides a high temperature resistant and wear resistant composite asphalt material, which is different from Example 1 in that the lignin sulfonate modified asphalt is replaced with base asphalt, specifically including the following contents: The high temperature resistant and wear resistant composite asphalt material comprises the following raw material components in percentage by weight: 75% lake asphalt, 5% lignin sulfonate modified asphalt, 6% waste ceramic particles and 14% oyster shell modified rubber particles.

[0051] The preparation method of the high temperature resistant and wear resistant composite asphalt material comprises the following steps: Step 1: weighing base asphalt according to the designed ratio, melting it at 130° C. to obtain a first asphalt component; weighing lake asphalt according to the designed ratio, melting it at 180° C. to obtain a second asphalt component; and mixing the first asphalt component and the second asphalt component evenly to obtain an asphalt component; Step 2: Keep the asphalt component at 175° C. for 40 minutes, add diatomaceous earth particles and oyster shell modified rubber particles according to the designed ratio, mix well, and obtain a high temperature resistant and wear resistant composite asphalt material.

[0052] The method for preparing the oyster shell modified rubber particles comprises the following steps: S1, ball milling 50 g of oyster shell at a speed of 700 rpm for 40 min, heating to 320° C., and keeping the temperature for 1.5 h to obtain pretreated oyster shell powder; S2, crushing 150g of waste rubber, mixing once at 150°C for 6min, adding 4.5g of anti-aging agent SP and the pretreated oyster shell powder, heating to 175°C for secondary mixing for 4min, and obtaining a rubber compound; S3. Add 3 g of accelerator NS and 3 g of sulfur to the rubber mixture for vulcanization, cooling, and granulation to obtain oyster shell modified rubber particles with a particle size of 150 μm.

[0053] The particle size of the waste ceramic particles is 80 μm.

[0054] In order to further reflect the technical effect of the present invention, the present invention conducted relevant performance tests on the composite asphalt materials obtained in Examples 1-3 and Comparative Examples 1-2, specifically including the following contents: "Technical Specifications for Asphalt Pavement Construction" (JTG F40-2004) stipulates that the composite asphalt materials obtained in Examples 1-3 and Comparative Examples 1-2 are subjected to softening point tests, dynamic stability tests, low temperature crack resistance tests and water stability tests; at the same time, the composite asphalt materials obtained in Examples 1-3 and Comparative Examples 1-2 are subjected to wear resistance tests and Kentaburg scattering tests. The wear resistance test is conducted using an MMW-1 microcomputer-controlled vertical universal friction and wear testing machine, wherein the test load is 80N, the rotation speed is 150rpm, and the test time is 1.5h. The test results are shown in Table 1.

[0055] Table 1 Test results of composite asphalt materials obtained in Examples 1-3 and Comparative Examples 1-2

[0056] It can be seen from Table 1 that the high temperature resistant and wear-resistant composite asphalt material provided by the present invention has excellent high temperature resistance, with a softening point of up to 83.2°C, and excellent low temperature resistance, with a low temperature bending failure strain of up to 3260μℇ. The composite asphalt material also has good wear resistance, with a scattering loss of only 1.1%, far lower than the standard requirement of 15%, and a low wear loss of only 0.60g. The high temperature resistant and wear-resistant composite asphalt material provided by the present invention effectively solves the problem of poor wear resistance and limited service life of asphalt pavements using lake asphalt as the main raw material in the prior art.

[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A high temperature and wear resistant composite asphalt material, Features: The raw material components include the following mass percentages: 25%-80% of lake asphalt, 3%-6% of lignin sulfonate modified asphalt, 5%-8% of waste ceramic particles and the balance of oyster shell modified rubber particles.

2. The high temperature and wear resistant composite asphalt material according to claim 1, Features: The preparation method of the oyster shell modified rubber particles comprises the following steps: S1, ball-milling the oyster shells, heating to 300-350° C., and keeping the temperature, to obtain pretreated oyster shell powder; S2, crushing the waste rubber, mixing it once at 120-160° C., adding an anti-aging agent and the pretreated oyster shell powder, heating it to 170-180° C. for secondary mixing to obtain a rubber compound; S3, adding an accelerator and a vulcanizing agent to the rubber mixture for vulcanization, cooling, and granulating to obtain oyster shell modified rubber particles.

3. The high temperature and wear resistant composite asphalt material according to claim 2, Features: In S1, the rotation speed of the ball mill is 600-800 rpm, and the time of the ball mill is 30-50 min; and / or In S1, the temperature is raised to 300-350°C by programmed heating at a heating rate of 10-15°C / min; and / or In S1, the insulation time is 1-2h.

4. The high temperature and wear resistant composite asphalt material according to claim 2, Features: In S2, the time of the first mixing is 5-8 min; and / or In S2, the secondary mixing time is 3-5 min; and / or In S2, the amount of the anti-aging agent added is 3%-5% of the mass of the waste rubber; and / or In S2, the mass ratio of the pretreated oyster shell powder to the waste rubber is 0.3:1-0.5:

1.

5. The high temperature and wear resistant composite asphalt material according to claim 2, Features: In S3, the amount of the accelerator added is 1%-3% of the mass of the rubber compound; and / or In S3, the amount of the vulcanizing agent added is 1%-3% of the mass of the rubber mixture.

6. The high temperature and wear resistant composite asphalt material according to claim 1, Features: The preparation method of the lignin sulfonate modified asphalt comprises the following steps: Step a, heating the lignin sulfonate modified asphalt to 130-160° C. to obtain a fluid asphalt component; Step b: adding lignin sulfonate to the mobile asphalt component, heating to 150-180° C., and stirring to obtain lignin sulfonate modified asphalt.

7. The high temperature and wear resistant composite asphalt material according to claim 6, Features: In step b, the amount of lignin sulfonate added is 5%-8% of the mass of the mobile asphalt component; and / or In step b, the rotation speed of the stirring treatment is 800-1000 rpm, and the time of the stirring treatment is 15-20 min.

8. The method for preparing the high temperature resistant and wear resistant composite asphalt material according to any one of claims 1 to 7, Features: The steps include: Step 1: weigh lignin sulfonate modified asphalt according to the designed ratio, melt it at 120-140° C. to obtain a first asphalt component; weigh lake asphalt according to the designed ratio, melt it at 165-190° C. to obtain a second asphalt component; mix the first asphalt component and the second asphalt component evenly to obtain an asphalt component; Step 2: Keep the asphalt component at 170-185° C., add waste ceramic particles and oyster shell modified rubber particles according to the designed ratio, mix them evenly, and obtain a high temperature resistant and wear resistant composite asphalt material.

9. The method for preparing the high temperature resistant and wear resistant composite asphalt material according to claim 8, Features: In step 2, the insulation time is 30-50 minutes.

10. Use of the high temperature and wear resistant composite asphalt material as claimed in any one of claims 1 to 7 or the high temperature and wear resistant composite asphalt material prepared by the preparation method of the high temperature and wear resistant composite asphalt material as claimed in claim 8 or 9 in the preparation of highway pavement materials.

Citation Information

Cited By

  • Composite asphalt material for road and preparation method thereof

    CN120795644A