Regenerated carbon black and preparation method thereof
By crushing, magnetic separation, sonication and oxidizing gas activation of waste tires, combined with nanocomposite fiber ball milling, regenerated carbon black with high dispersion and high binding strength was prepared, and the poor dispersion of carbon black in the prior art was solved. Combined with the problem of insufficient strength, the mechanical properties of the matrix material have been significantly improved.
Patent Information
- Application Number
- CN202411193983.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, recycled carbon black has poor dispersion and is prone to agglomeration during the preparation of plastics, resulting in poor comprehensive mechanical properties of the matrix material and limited application range.
Use waste tires as raw materials to prepare regenerated carbon black through steps such as crushing, magnetic separation, ultrasonic treatment, oxidizing gas activation and ball milling, and ball milling is combined with nanocomposite fibers to enhance the interface effect and bonding strength between the carbon black and the matrix material.
It effectively improves the dispersion and bonding strength of carbon black, enhances the mechanical properties of the matrix material, and makes its application more widely.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber reinforcement, in particular to regenerated carbon black and a preparation method thereof. Background Art
[0002] Carbon black is a light, loose, extremely fine black powder with a large specific surface area. According to the performance of carbon black, it can be divided into conductive carbon black, reinforcing carbon black, wear-resistant carbon black, etc. Due to the low density and large specific surface area of carbon black, it is very easy to agglomerate. Especially in the process of plastic processing, carbon black cannot be well dispersed in the plastic, which also limits its performance. Although the prior art adds a dispersant to disperse carbon black during the preparation of plastics, in the actual production process, the dispersant needs to be re-measured and added, which increases the operation steps; most importantly, the dispersants added in the existing plastic preparation process are all conventional dispersants, which cannot disperse carbon black in the plastic to the greatest extent, so more carbon black needs to be added to achieve the desired effect, which correspondingly increases the cost of plastic products.
[0003] For example, the invention patent with the announcement number CN113667328A discloses a regenerated carbon black and its preparation method and application, including the following steps: a. subjecting the cracked carbon black to a temperature-raising activation treatment to obtain the activated cracked carbon black; b. subjecting the cracked carbon black obtained in step a to a temperature-lowering treatment to obtain the regenerated carbon black. The present invention takes into account the three major reinforcement factors of the cracked carbon black, namely, the ash content, particle size and surface colloid layer, and combines the heating and cooling processes with the aid of an oxidizing atmosphere to achieve the decomposition and removal of the surface colloid layer and organic macromolecules of the cracked carbon black, and retains the reinforcing activity of the original cracked carbon black to the greatest extent; although the technical solution provided by the patent can obtain low-cost regenerated carbon black with high reinforcing performance that meets the needs of rubber manufacturing, and realizes the recycling of solid waste resources, the prepared regenerated carbon black is easy to agglomerate, has poor dispersibility, and has a weak interface with the matrix material and poor bonding strength, resulting in poor comprehensive mechanical properties of the matrix material and a relatively limited scope of application. Summary of the invention
[0004] In view of the problems existing in the prior art, the object of the present invention is to provide a regenerated carbon black and a preparation method thereof.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing regenerated carbon black specifically comprises the following steps:
[0007] S1. After the waste tires are crushed, they are mixed with a desulfurizer, a mixed acid is added, and the mixture is placed in a reactor for reaction, and the product is activated under an oxidizing gas to obtain a crude carbon black product;
[0008] S2. The crude carbon black is subjected to magnetic separation treatment in a magnetic separator for 2-6 minutes, mixed with a desulfurizer and subjected to ultrasonic treatment for 10-20 seconds, heated to 95-120°C for treatment for 3-7 minutes, then cooled to room temperature, mixed with an equal mass of electrical nanomaterials and ball milled to obtain the desired finished regenerated carbon black.
[0009] As a further preferred embodiment of the present invention, the mass ratio of the waste tire to the desulfurizer is 1:(1.0-1.2);
[0010] The mass volume ratio of the waste tire to the mixed acid is (5-6): (0.1-0.7);
[0011] The preparation method of the desulfurizing agent is as follows: by weight, 2-6 parts of N-methyldiethanolamine, 1-3 parts of rosin, and 3-5 parts of waste oil are mixed at a temperature of 50-55° C., and ultrasonically treated at 50-80 Hz for 10-30 seconds, and then 0.1-0.6 parts of iron oxide, 0.01-0.05 parts of magnesium bicarbonate, and 0.03-0.08 parts of sodium bicarbonate are added thereto, and stirred at 500-800 r / min for 10-30 minutes.
[0012] The mixed acid is prepared by mixing equal volumes of hydrochloric acid and nitric acid, to which is added 0.1-0.3 times the volume of nitric acid permanganate.
[0013] As a further preferred embodiment of the present invention, the reaction in the reactor is specifically as follows: first, the temperature is raised to 75-85°C, and the temperature is kept constant for 20-30 minutes, and then the temperature is raised to 110-120°C at a rate of 2-6°C / min, and the pressure in the reactor is adjusted to 5-8MPa, and the temperature is raised to 250-265°C at a rate of 1-3°C / min, and the temperature is kept constant for 10-30 minutes, and the temperature is raised to 490-520°C in 20-30 seconds for 20-30 minutes, and then the temperature is lowered to room temperature in 10-20 minutes.
[0014] As a further preferred embodiment of the present invention, the temperature of the activation treatment is 600-750°C, and the activation time is 10-30min;
[0015] The oxidizing gas is selected from at least one of oxygen, carbon dioxide and water vapor;
[0016] The flow rate of the oxidizing gas is 0.1-0.3 L / s.
[0017] As a further preferred embodiment of the present invention, the mass ratio of the crude carbon black to the desulfurizing agent is 1:(0.002-0.006);
[0018] The frequency of the ultrasonic treatment is 200-300 Hz;
[0019] The ball mill has a rotation speed of 100-300 r / min and a ball milling time of 1-2 h.
[0020] As a further preferred embodiment of the present invention, the preparation method of the electrical nanomaterial is as follows:
[0021] 1) 1-5 g of nanocomposite fiber and 3-6 mL of ammonia water are sequentially added to 40-60 mL of ethanol aqueous solution, stirred at 500-800 r / min for 1-2 h, and then heated to 52-58 ° C to obtain a suspension, 3-5 mL of tetraethyl orthosilicate is dissolved in 8-15 mL of ethanol aqueous solution, shaken and mixed evenly, and then added dropwise to the suspension for reaction for 2-5 h;
[0022] 2) After the reaction is completed, epichlorohydrin is added to the reaction solution, and the reaction is stirred at 52-58° C. for 2-5 hours, and then 3-dimethylaminopropylamine is added, and the reaction is continued at a constant temperature for 2-5 hours. After natural cooling, the product is centrifuged and washed to neutrality, and then dried to obtain an electrical nanomaterial.
[0023] As a further preferred embodiment of the present invention, the concentration of the aqueous ammonia is 22-25wt%;
[0024] The concentration of the ethanol aqueous solution is 95-98wt%;
[0025] The molar ratio of tetraethyl orthosilicate, epichlorohydrin and 3-dimethylaminopropylamine is 1:(2.0-2.5):(2.0-2.5).
[0026] As a further preferred embodiment of the present invention, the preparation method of the nanocomposite fiber is as follows:
[0027] 1) 50-100 mg of terephthalic acid is dissolved in a mixed solution A consisting of 10-20 mL of N,N-dimethylformamide and 5-10 mL of acetonitrile, and placed in a container as a bottom solution, and then a mixed solution B consisting of 5-10 mL of N,N-dimethylformamide and 5-10 mL of acetonitrile is used as a separator in the container, and then 25-50 mg of cobalt acetate tetrahydrate and 25-50 mg of nickel acetate tetrahydrate are dissolved in a mixed solution C consisting of 5-10 mL of N,N-dimethylformamide and 10-20 mL of acetonitrile as the top layer of the container, and then placed in a 30-35° C. thermostat for reaction for 24-30 hours. After the reaction is completed, it is repeatedly washed with N,N-dimethylformamide, the product is collected after filtration, and after drying, a nanosheet precursor is obtained;
[0028] 2) After mixing the nanosheet precursor with dicyandiamide, add it to N,N-dimethylformamide, stir it with magnetic force at a constant temperature of 50-55°C, then add polyacrylonitrile, stir it thoroughly to obtain a spinning precursor, and then load it into a micro-injection pump with an injection speed of 1-3mL / h. Electrospinning is performed at 10-15kV, the distance between the collector and the syringe needle is 10-15cm, the rotation speed is 60-100r / min, and the obtained fiber is heated from room temperature to 700-750°C at a rate of 4-6°C / min under an argon atmosphere, and carbonized for 2-5h to obtain a nano-composite fiber.
[0029] As a further preferred embodiment of the present invention, in the spinning precursor, the usage ratio of the nanosheet precursor, dicyandiamide, N,N-dimethylformamide and polyacrylonitrile is (8-9) g: (1-2) g: (60-100) mL: (40-50) g.
[0030] A regenerated carbon black is prepared by the method.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] In the present invention, a three-layer solution method is adopted, cobalt acetate tetrahydrate and nickel acetate tetrahydrate are used to provide metal cations, terephthalic acid is used as an organic ligand, N,N-dimethylformamide and acetonitrile are used as organic solvents, and a nanosheet precursor with a layered structure is obtained through reaction. Then, an electrostatic spinning technology is used to electrostatically spin a two-dimensional layered nanosheet precursor, a nitrogen source dicyandiamide and a polyacrylonitrile polymer, and a nanocomposite fiber is generated through a one-step heat treatment. The inorganic nitrogen source dicyandiamide is added to increase the nitrogen concentration, which can promote the extensive formation of active sites on the surface of the nanocomposite fiber after the heat treatment, thereby effectively enhancing the activity of carbon black, helping to enhance the interface effect between the carbon black and the matrix material, and at the same time, the nanocomposite fiber After being added to the matrix material, on the one hand, a mesh support structure can be constructed to disperse and transfer stress, thereby enhancing the mechanical properties of the matrix material. At the same time, a larger contact area can be formed between the matrix material to enhance the bonding strength between the two, so that it can stably exist in the matrix material without migration. At the same time, in order to avoid agglomeration between the nano-composite fibers, the nano-composite fibers are surface treated in the present invention to obtain electrical nano-materials. Cationic functional groups are covalently grafted on the surface to give them certain characteristics of quaternary ammonium salts and good dispersibility, thereby avoiding the occurrence of agglomeration. At the same time, the surface carries a positive charge, and under the action of electrostatics, they repel each other, so they can be highly dispersed.
[0033] In the present invention, waste tires are used as raw materials, mixed with a desulfurizer, and then mixed with a mixed acid, heated to react, and then subjected to magnetic separation, desulfurization, heated ultrasonic catalytic reaction, and oxidizing gas activation treatment, so that impurities in the waste tires are removed in large quantities, the quality of carbon black is improved, and the obtained carbon black crude product is ball-milled and mixed with an electrical nano material to combine the two together, which increases the dispersibility of the carbon black and strengthens the interface between the carbon black and the matrix material, thereby improving the bonding strength, thereby enhancing the mechanical properties of the matrix material and making it more widely used. DETAILED DESCRIPTION
[0034] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Example 1
[0036] A method for preparing regenerated carbon black specifically comprises the following steps:
[0037] 1) After the waste tire is crushed into 20 mesh particles, it is mixed with the desulfurizer in a mass ratio of 1:1, and then the frequency is controlled by an ultrasonic processor to be 1200Hz for 10s, and then the mixed acid is added according to the mass volume ratio of the waste tire to the mixed acid of 5:0.1, and placed in a reactor, and the temperature is adjusted to 75°C. After the temperature is kept constant for 20min, it is heated to 110°C at a heating rate of 2°C / min, and the pressure in the reactor is adjusted to 5MPa, and the temperature is further increased to 250°C at a rate of 1°C / min, and the temperature is kept constant for 10min, and the temperature is increased to 490°C in 20s for 20min, and then it is cooled to room temperature in 10min, and then the obtained product is activated at 600°C for 10min under an oxygen atmosphere, and the oxygen flow rate is 0.1L / s to obtain a crude carbon black product;
[0038] 2) The crude carbon black is sent to a magnetic separator for magnetic separation for 2 minutes, mixed with a desulfurizer at a mass ratio of 1:0.002, sent to an ultrasonic wave at a frequency of 200 Hz for 10 seconds, heated to 95°C for 3 minutes, then cooled to room temperature, mixed with an equal mass of electrical nanomaterials, and ball milled at a speed of 100 r / min for 1 hour to obtain the desired finished regenerated carbon black;
[0039] The preparation method of the desulfurizer is as follows: by weight, 2 parts of N-methyldiethanolamine, 1 part of rosin, and 3 parts of waste oil are mixed at a temperature of 50°C, and ultrasonically treated at 50 Hz for 10 seconds, and then 0.1 parts of iron oxide, 0.01 parts of magnesium bicarbonate, and 0.03 parts of sodium bicarbonate are added thereto, and stirred at 500 r / min for 10 minutes.
[0040] The mixed acid is prepared by mixing equal volumes of hydrochloric acid and nitric acid, to which is added 0.1 times the volume of nitric acid permanganate.
[0041] The preparation method of the above-mentioned electrical nanomaterial is as follows:
[0042] 1) 50 mg of terephthalic acid was dissolved in a mixed solution A consisting of 10 mL of N, N-dimethylformamide and 5 mL of acetonitrile, and placed in a container as a bottom solution, and then a mixed solution B consisting of 5 mL of N, N-dimethylformamide and 5 mL of acetonitrile was used as a separator in the container, and then 25 mg of cobalt acetate tetrahydrate and 25 mg of nickel acetate tetrahydrate were dissolved in a mixed solution C consisting of 5 mL of N, N-dimethylformamide and 10 mL of acetonitrile as the top layer of the container, and then placed in a 30° C. thermostat for reaction for 24 hours. After the reaction was completed, it was repeatedly washed with N, N-dimethylformamide, the product was collected after filtration, and after drying, a nanosheet precursor was obtained;
[0043] 2) After mixing 8 g of the nanosheet precursor with 1 g of dicyandiamide, add it to 60 mL of N,N-dimethylformamide, stir it with a constant temperature magnetic force at 50 ° C, then add 40 g of polyacrylonitrile, stir it thoroughly to obtain a spinning precursor, and then load it into a micro-injection pump, the injection speed is 1 mL / h, electrospinning is performed at 10 kV, the distance between the collector and the syringe needle is 10 cm, the rotation speed is 60 r / min, and the obtained fiber is heated from room temperature to 700 ° C at a rate of 4 ° C / min in an argon atmosphere, and carbonized for 2 h to obtain a nanocomposite fiber;
[0044] 3) 1 g of nanocomposite fiber and 3 mL of 22 wt% ammonia water were sequentially added to 40 mL of 95 wt% ethanol aqueous solution, stirred at 500 r / min for 1 h, and then heated to 52° C. to obtain a suspension, 3 mL of tetraethyl orthosilicate was dissolved in 8 mL of 95 wt% ethanol aqueous solution, oscillated and mixed, and then added dropwise to the suspension for 2 h;
[0045] 4) After the reaction is completed, epichlorohydrin is added to the reaction solution according to the molar ratio of tetraethyl orthosilicate, epichlorohydrin and 3-dimethylaminopropylamine being 1:2:2, and the reaction is stirred at 52°C for 2 hours, and then 3-dimethylaminopropylamine is added, and the reaction is continued at a constant temperature for 2 hours. After natural cooling, the product is centrifuged and washed to neutrality, and then dried to obtain an electrical nanomaterial.
[0046] Example 2
[0047] A method for preparing regenerated carbon black specifically comprises the following steps:
[0048] 1) After the waste tire is crushed into 30 mesh particles, it is mixed with the desulfurizer at a mass ratio of 1:1.1, and then the frequency is controlled by an ultrasonic processor to be 1300Hz for 20s, and then the mixed acid is added according to the mass volume ratio of the waste tire to the mixed acid of 5.5:0.4, and placed in a reactor, and the temperature is adjusted to 80°C. After the temperature is kept constant for 25min, it is heated to 115°C at a heating rate of 5°C / min, and the pressure in the reactor is adjusted to 7MPa, and the temperature is further increased to 255°C at a rate of 2°C / min, and the temperature is kept constant for 20min, and the temperature is increased to 500°C in 25s for 25min, and then it is cooled to room temperature in 15min, and then the obtained product is activated at 700°C for 20min under an oxygen atmosphere, and the oxygen flow rate is 0.2L / s to obtain a crude carbon black product;
[0049] 2) The crude carbon black is sent to a magnetic separator for magnetic separation for 5 minutes, mixed with a desulfurizer at a mass ratio of 1:0.005, sent to an ultrasonic wave at a frequency of 300 Hz for 15 seconds, heated to 110°C for 5 minutes, then cooled to room temperature, mixed with an equal mass of electrical nanomaterials, and ball milled at a speed of 200 r / min for 1.5 hours to obtain the desired finished regenerated carbon black;
[0050] The preparation method of the desulfurizer is as follows: 5 parts of N-methyldiethanolamine, 2 parts of rosin, and 4 parts of waste oil are mixed at a temperature of 52°C, and ultrasonically treated at 70 Hz for 20 seconds, and then 0.5 parts of iron oxide, 0.03 parts of magnesium bicarbonate, and 0.05 parts of sodium bicarbonate are added thereto, and stirred at 700 r / min for 20 minutes.
[0051] The mixed acid is prepared by mixing equal volumes of hydrochloric acid and nitric acid, to which is added 0.2 times the volume of nitric acid permanganate.
[0052] The preparation method of the above-mentioned electrical nanomaterial is as follows:
[0053] 1) 80 mg of terephthalic acid was dissolved in a mixed solution A consisting of 15 mL of N, N-dimethylformamide and 7 mL of acetonitrile, and placed in a container as a bottom solution, and then a mixed solution B consisting of 7 mL of N, N-dimethylformamide and 7 mL of acetonitrile was used as a separator in the container, and then 40 mg of cobalt acetate tetrahydrate and 40 mg of nickel acetate tetrahydrate were dissolved in a mixed solution C consisting of 7 mL of N, N-dimethylformamide and 15 mL of acetonitrile as the top layer of the container, and then placed in a 32° C. thermostat for reaction for 28 hours. After the reaction was completed, it was repeatedly washed with N, N-dimethylformamide, the product was collected after filtration, and after drying, a nanosheet precursor was obtained;
[0054] 2) 8.5 g of the nanosheet precursor was mixed with 1.5 g of dicyandiamide, added to 80 mL of N,N-dimethylformamide, and magnetically stirred at a constant temperature of 52 ° C. Then, 45 g of polyacrylonitrile was added and stirred thoroughly to obtain a spinning precursor, which was then loaded into a micro-injection pump at an injection speed of 2 mL / h. Electrospinning was performed at 12 kV, with the collector being 12 cm away from the syringe needle, and the rotation speed was 80 r / min. The obtained fiber was heated from room temperature to 720 ° C at a rate of 5 ° C / min under an argon atmosphere, and carbonized for 3 h to obtain a nanocomposite fiber;
[0055] 3) 3 g of nanocomposite fiber and 5 mL of 23 wt% ammonia water were sequentially added to 50 mL of 96 wt% ethanol aqueous solution, stirred at 700 r / min for 1.5 h, and then heated to 55° C. to obtain a suspension, 4 mL of tetraethyl orthosilicate was dissolved in 12 mL of 96 wt% ethanol aqueous solution, oscillated and mixed, and then added dropwise to the suspension for 3 h;
[0056] 4) After the reaction is completed, epichlorohydrin is added to the reaction solution according to the molar ratio of tetraethyl orthosilicate, epichlorohydrin and 3-dimethylaminopropylamine of 1:2.3:2.3, and the reaction is stirred at 55°C for 3 hours. Then 3-dimethylaminopropylamine is added and the reaction is continued at a constant temperature for 3 hours. After natural cooling, the product is centrifuged and washed to neutrality, and then dried to obtain an electrical nanomaterial.
[0057] Example 3
[0058] A method for preparing regenerated carbon black specifically comprises the following steps:
[0059] 1) After the waste tire is crushed into 30 mesh particles, it is mixed with the desulfurizer at a mass ratio of 1:1.2, and then the ultrasonic processor is used to control the frequency to 1500Hz for 30s, and then the mixed acid is added according to the mass volume ratio of the waste tire to the mixed acid of 6:0.7, and placed in a reactor, and the temperature is adjusted to 85°C. After the temperature is kept constant for 30min, it is heated to 120°C at a heating rate of 6°C / min, and the pressure in the reactor is adjusted to 8MPa, and the temperature is further increased to 265°C at a rate of 3°C / min, and the temperature is kept constant for 30min, and the temperature is increased to 520°C in 30s for 30min, and then it is cooled to room temperature in 20min, and then the obtained product is activated at 750°C for 30min under an oxygen atmosphere, and the oxygen flow rate is 0.3L / s to obtain a crude carbon black product;
[0060] 2) The crude carbon black is sent to a magnetic separator for magnetic separation for 6 minutes, mixed with a desulfurizer at a mass ratio of 1:0.006, sent to an ultrasonic wave at a frequency of 300 Hz for 20 seconds, heated to 120°C for 7 minutes, then cooled to room temperature, mixed with an equal mass of electrical nanomaterials, and ball milled at a speed of 300 r / min for 2 hours to obtain the desired finished regenerated carbon black;
[0061] The preparation method of the desulfurizer is as follows: by weight, 6 parts of N-methyldiethanolamine, 3 parts of rosin, and 5 parts of waste oil are mixed at a temperature of 55°C, and ultrasonically treated at 80 Hz for 30 seconds, and then 0.6 parts of iron oxide, 0.05 parts of magnesium bicarbonate, and 0.08 parts of sodium bicarbonate are added thereto, and stirred at 800 r / min for 30 minutes.
[0062] The mixed acid is prepared by mixing equal volumes of hydrochloric acid and nitric acid, to which is added 0.3 times the volume of nitric acid permanganate.
[0063] The preparation method of the above-mentioned electrical nanomaterial is as follows:
[0064] 1) 100 mg of terephthalic acid is dissolved in a mixed solution A consisting of 20 mL of N,N-dimethylformamide and 10 mL of acetonitrile, and placed in a container as a bottom solution, and then a mixed solution B consisting of 10 mL of N,N-dimethylformamide and 10 mL of acetonitrile is used as a separator in the container, and then 50 mg of cobalt acetate tetrahydrate and 50 mg of nickel acetate tetrahydrate are dissolved in a mixed solution C consisting of 10 mL of N,N-dimethylformamide and 20 mL of acetonitrile as the top layer of the container, and then placed in a 35° C. thermostat for reaction for 30 hours. After the reaction is completed, it is repeatedly washed with N,N-dimethylformamide, the product is collected after filtration, and after drying, a nanosheet precursor is obtained;
[0065] 2) After mixing 9 g of the nanosheet precursor with 2 g of dicyandiamide, add it to 100 mL of N,N-dimethylformamide, stir it with a constant temperature magnetic force at 55 ° C, then add 50 g of polyacrylonitrile, stir it thoroughly to obtain a spinning precursor, and then load it into a micro-injection pump, the injection speed is 3 mL / h, electrospinning is performed at 15 kV, the distance between the collector and the syringe needle is 15 cm, the rotation speed is 100 r / min, and the obtained fiber is heated from room temperature to 750 ° C at a rate of 6 ° C / min in an argon atmosphere, and carbonized for 5 h to obtain a nanocomposite fiber;
[0066] 3) 5 g of nanocomposite fiber and 6 mL of 25 wt% ammonia water were sequentially added to 60 mL of 98 wt% ethanol aqueous solution, stirred at 800 r / min for 2 h, and then heated to 58° C. to obtain a suspension, 5 mL of tetraethyl orthosilicate was dissolved in 15 mL of 98 wt% ethanol aqueous solution, oscillated and mixed, and then added dropwise to the suspension for 5 h;
[0067] 4) After the reaction is completed, epichlorohydrin is added to the reaction solution according to the molar ratio of tetraethyl orthosilicate, epichlorohydrin and 3-dimethylaminopropylamine being 1:2.5:2.5, and the reaction is stirred at 58°C for 5 hours, and then 3-dimethylaminopropylamine is added, and the reaction is continued at a constant temperature for 5 hours. After natural cooling, the product is centrifuged and washed to neutrality, and then dried to obtain an electrical nanomaterial.
[0068] Comparative Example 1: This comparative example is basically the same as Example 1, except that it does not contain electrical nanomaterials.
[0069] Comparative Example 2: This comparative example is basically the same as Example 1, except that step 1) is omitted in the preparation of the electrical nanomaterial.
[0070] Comparative Example 3: This comparative example is basically the same as Example 1, except that step 2) is omitted in the preparation of the electrical nanomaterial.
[0071] Comparative Example 4: This comparative example is basically the same as Example 1, except that in the preparation of the electrical nanomaterial, steps 1)-2) are omitted.
[0072] Comparative Example 5: This comparative example is basically the same as Example 1, except that in the preparation of the electrical nanomaterial, steps 3)-4) are omitted.
[0073] Test experiment:
[0074] The regenerated carbon black samples were obtained by the methods provided in Examples 1-3 and Comparative Examples 1-5, and then applied to the sidewall rubber for experiments. The amount of carbon black was controlled to be 20 parts by weight per 100 parts by weight of rubber. The results are shown in Table 1.
[0075] Table 1
[0076] Example 1 Example 2 Example 3 Comparative Example 1 Tensile strength MPa 24.3 24.7 24.6 19.7 Tear strength KN / m 153 159 157 120 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Tensile strength MPa 22.5 22.9 21.3 20.6 Tear strength KN / m 138 140 132 128
[0077] It can be seen from Table 1 that the regenerated carbon black prepared in the present invention can effectively enhance the mechanical properties of the base material, making its application more extensive.
[0078] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing regenerated carbon black, characterized in that: The specific steps include: S1. After the waste tires are crushed, they are mixed with a desulfurizer, a mixed acid is added, and the mixture is placed in a reactor for reaction, and the product is activated under an oxidizing gas to obtain a crude carbon black product; S2. The crude carbon black is subjected to magnetic separation treatment in a magnetic separator for 2-6 minutes, mixed with a desulfurizer and subjected to ultrasonic treatment for 10-20 seconds, heated to 95-120°C for treatment for 3-7 minutes, then cooled to room temperature, mixed with an equal mass of electrical nanomaterials and ball milled to obtain the desired finished regenerated carbon black.
2. The method for preparing regenerated carbon black according to claim 1, characterized in that: The mass ratio of the waste tire to the desulfurizer is 1:(1.0-1.2); The mass volume ratio of the waste tire to the mixed acid is (5-6): (0.1-0.7); The preparation method of the desulfurizing agent is as follows: by weight, 2-6 parts of N-methyldiethanolamine, 1-3 parts of rosin, and 3-5 parts of waste oil are mixed at a temperature of 50-55° C., and ultrasonically treated at 50-80 Hz for 10-30 seconds, and then 0.1-0.6 parts of iron oxide, 0.01-0.05 parts of magnesium bicarbonate, and 0.03-0.08 parts of sodium bicarbonate are added thereto, and stirred at 500-800 r / min for 10-30 minutes. The mixed acid is prepared by mixing equal volumes of hydrochloric acid and nitric acid, to which is added 0.1-0.3 times the volume of nitric acid permanganate.
3. The method for preparing regenerated carbon black according to claim 1, characterized in that: The reaction in the reactor is specifically as follows: firstly heating to 75-85°C, keeping the temperature constant for 20-30min, then heating to 110-120°C at a rate of 2-6°C / min, adjusting the pressure in the reactor to 5-8MPa, heating to 250-265°C at a rate of 1-3°C / min, keeping the temperature constant for 10-30min, heating to 490-520°C in 20-30s for 20-30min, and then cooling to room temperature in 10-20min.
4. The method for preparing regenerated carbon black according to claim 1, characterized in that: The activation treatment temperature is 600-750°C, and the activation time is 10-30min; The oxidizing gas is selected from at least one of oxygen, carbon dioxide and water vapor; The flow rate of the oxidizing gas is 0.1-0.3 L / s.
5. The method for preparing regenerated carbon black according to claim 1, characterized in that: The mass ratio of the crude carbon black to the desulfurizing agent is 1:(0.002-0.006); The frequency of the ultrasonic treatment is 200-300 Hz; The ball mill has a rotation speed of 100-300 r / min and a ball milling time of 1-2 h.
6. The method for preparing regenerated carbon black according to claim 1, characterized in that: The preparation method of the electrical nanomaterial is as follows: 1) 1-5 g of nanocomposite fiber and 3-6 mL of ammonia water are sequentially added to 40-60 mL of ethanol aqueous solution, stirred at 500-800 r / min for 1-2 h, and then heated to 52-58 ° C to obtain a suspension, 3-5 mL of tetraethyl orthosilicate is dissolved in 8-15 mL of ethanol aqueous solution, shaken and mixed evenly, and then added dropwise to the suspension for reaction for 2-5 h; 2) After the reaction is completed, epichlorohydrin is added to the reaction solution, and the reaction is stirred at 52-58° C. for 2-5 hours, and then 3-dimethylaminopropylamine is added, and the reaction is continued at a constant temperature for 2-5 hours. After natural cooling, the product is centrifuged and washed to neutrality, and then dried to obtain an electrical nanomaterial.
7. The method for preparing regenerated carbon black according to claim 6, characterized in that: The concentration of the aqueous ammonia is 22-25wt%; The concentration of the ethanol aqueous solution is 95-98wt%; The molar ratio of tetraethyl orthosilicate, epichlorohydrin and 3-dimethylaminopropylamine is 1:(2.0-2.5):(2.0-2.5).
8. The method for preparing regenerated carbon black according to claim 6, characterized in that: The preparation method of the nanocomposite fiber is as follows: 1) 50-100 mg of terephthalic acid is dissolved in a mixed solution A consisting of 10-20 mL of N,N-dimethylformamide and 5-10 mL of acetonitrile, and placed in a container as a bottom solution, and then a mixed solution B consisting of 5-10 mL of N,N-dimethylformamide and 5-10 mL of acetonitrile is used as a separator in the container, and then 25-50 mg of cobalt acetate tetrahydrate and 25-50 mg of nickel acetate tetrahydrate are dissolved in a mixed solution C consisting of 5-10 mL of N,N-dimethylformamide and 10-20 mL of acetonitrile as the top layer of the container, and then placed in a 30-35° C. thermostat for reaction for 24-30 hours. After the reaction is completed, it is repeatedly washed with N,N-dimethylformamide, the product is collected after filtration, and after drying, a nanosheet precursor is obtained; 2) After mixing the nanosheet precursor with dicyandiamide, add it to N,N-dimethylformamide, stir it with magnetic force at a constant temperature of 50-55°C, then add polyacrylonitrile, stir it thoroughly to obtain a spinning precursor, and then load it into a micro-injection pump with an injection speed of 1-3mL / h. Electrospinning is performed at 10-15kV, the distance between the collector and the syringe needle is 10-15cm, the rotation speed is 60-100r / min, and the obtained fiber is heated from room temperature to 700-750°C at a rate of 4-6°C / min under an argon atmosphere, and carbonized for 2-5h to obtain a nano-composite fiber.
9. The method for preparing regenerated carbon black according to claim 8, characterized in that: In the spinning precursor, the usage ratio of the nanosheet precursor, dicyandiamide, N,N-dimethylformamide and polyacrylonitrile is (8-9) g: (1-2) g: (60-100) mL: (40-50) g.
10. A regenerated carbon black, characterized in that The method is prepared by any one of claims 1 to 9.