Preparation method of heavy anti-corrosion coating of grafted modified graphene
By treating graphene and nano-cerium oxide aqueous solution under a nitrogen atmosphere, combining zinc powder and epoxy resin, a heavy anticorrosion coating with grafted modified graphene was prepared, which solved the problem of dispersion of graphene in the coating and significantly improved the Anticorrosion effect and adhesion are suitable for long-term protection in harsh environments.
Patent Information
- Application Number
- CN202411277770.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-12
AI Technical Summary
Graphene is difficult to disperse in the coating, resulting in agglomeration and affecting the water seepage resistance of the paint film. A method for preparing heavy anticorrosion coatings with grafted modified graphene is urgently needed to improve the anticorrosion effect.
3-isocyanate propyltrimethoxysilane is mixed with graphene oxide under a nitrogen atmosphere, and after sonication, N,N-dimethylformamide and nano-cerium oxide aqueous solution are added to form isocyanate-modified graphene oxide, and A modified graphene-zinc composite powder was synthesized with zinc powder, combined with epoxy resin and modified filler, and a heavy anticorrosion coating with grafted modified graphene was prepared by stirring and grinding.
It significantly improves the anticorrosion effect and adhesion of the coating, forms a dense coating, enhances the anticorrosion performance, and is suitable for long-term protection in harsh environments.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coatings, and in particular relates to a method for preparing a heavy-duty anti-corrosion coating of grafted modified graphene. Background Art
[0002] Heavy-duty coating is a high-performance anti-corrosion coating. Compared with conventional anti-corrosion coating, it can provide long-term protection in more harsh corrosive environments and has a longer service life. The main characteristics of this coating include: Long-term anti-corrosion life: It can be used for more than 10 or 15 years in chemical atmosphere and marine environment, and can be used for more than 5 years in acid, alkali, salt and solvent media under certain temperature conditions. Thick film: The dry film thickness of heavy-duty coating is usually more than 200μm or 300μm, and some can even reach 500μm to 1000μm, or even 2000μm. Wide range of applications: Applicable to emerging marine engineering, modern transportation, energy industry, large industrial enterprises and municipal facilities.
[0003] As a new type of anti-corrosion material, graphene is added to conventional anti-corrosion coatings, which has the characteristics of good flexibility, strong adhesion, good water resistance, high hardness, etc. It can be widely used in coating protection in the fields of marine engineering, petroleum and petrochemicals, transportation, industrial equipment and containers. Graphene has a large specific surface area and is difficult to disperse directly in the coating. It is easy to agglomerate, which will affect the ability of the paint film to resist water penetration.
[0004] Therefore, there is an urgent need for a method for preparing a heavy-duty anti-corrosion coating of grafted modified graphene. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a heavy-duty anti-corrosion coating of grafted modified graphene.
[0006] In order to achieve the above object, the present invention provides the following technical solutions: A method for preparing a heavy-duty anti-corrosion coating of grafted modified graphene, the preparation method comprising the following steps: (1) Under a nitrogen atmosphere, 1 part by mass of 3-isocyanate propyl trimethoxy silane and 0.13-0.16 part by mass of graphene oxide are mixed, ultrasonicated for 20-25 min, 60-65 parts by mass of N, N-dimethylformamide are added, stirred at 102-105° C. for 2-3 h, centrifuged, and the solid is freeze-dried to obtain isocyanate-modified graphene oxide; 10 parts by mass of isocyanate-modified filler are added to 60-63 parts by mass of ethanol, and then a nano-cerium oxide aqueous solution with a mass percentage of 2.5-3.0wt% is added dropwise; after the addition is completed, stirring is continued at 56-58° C. for 2-3 h, centrifuged, and the solid is freeze-dried to obtain grafted modified graphene; (2) Add zinc powder to a three-necked flask, add toluene diisocyanate and isopropanol, add grafted modified graphene, and ultrasonically disperse for 15-20 minutes under nitrogen protection. After dispersion, heat to 90-100°C, stir and react for 1-2 hours, filter, and dry the residue in a vacuum drying oven to obtain modified graphene-zinc composite powder; (3) Select 34-38 parts of epoxy resin, 8-10 parts of modified filler, 10-15 parts of solvent, 1-2 parts of leveling agent, 1-2 parts of dispersant, 0.1-0.5 parts of defoaming agent and 1-1.3 parts of silane coupling agent by weight, mix them and add them to a stirring tank in sequence, start stirring, control the stirring speed to 300-400r / min, add 10-20 parts of modified graphene-zinc composite powder to the stirring tank in 3-5 times, continue stirring for 20-25 minutes, then add it to a grinder and grind it until the particle size is less than 50μm, and obtain epoxy resin slurry, which is component A; (4) In parts by weight, the composition comprises: 10-13 parts of isophorone diamine, 2-3 parts of dibutyl phthalate and 5-8 parts of n-butanol, which are mixed uniformly to obtain component B; (5) Component A and component B are packaged separately and mixed evenly at a mass ratio of 6-9:1 when used to obtain a heavy-duty anti-corrosion coating of grafted modified graphene.
[0007] Furthermore, the mass ratio of isocyanate-modified graphene oxide to nano-cerium oxide is 10:(1-3).
[0008] Furthermore, the mass ratio of the grafted modified graphene to the zinc powder is 1:20-23.
[0009] Furthermore, the epoxy resin in step (3) is one of bisphenol A epoxy resin, novolac epoxy resin or silicone epoxy resin.
[0010] Furthermore, the solvent in step (3) is a mixture of butyl acetate and n-butanol in a mass ratio of 1:5.
[0011] Furthermore, the leveling agent in step (3) is the leveling agent BYK-333; the defoaming agent is one of tributyl phosphate and dimethyl silicone oil; and the silane coupling agent is KH-560.
[0012] Furthermore, the dispersant in step (3) is one or more of polyethylene wax, polyvinyl pyrrolidone, sodium carboxymethyl cellulose, and polyethylene glycol.
[0013] Furthermore, the preparation method of the modified filler includes the following steps: mixing filler, 55wt% ethanol aqueous solution and silane coupling agent KH550 in a mass ratio of 1:6-8:0.02-0.03, stirring and reacting at 60-65°C for 2-4h, filtering the solid, washing and drying to obtain the modified filler.
[0014] Furthermore, the filler comprises nano-aluminum oxide, nano-silicon nitride and nano-lanthanum oxide in a mass ratio of 1:1.3-1.5:0.5-0.7.
[0015] Furthermore, the particle size of nano-alumina is 200-300nm and the specific surface area is 40-55m 2 / g; the particle size of nano silicon nitride is 50-100nm, and the specific surface area is 30-43m 2 / g; the particle size of nano lanthanum oxide is 120-160nm, and the specific surface area is 15-35m 2 / g.
[0016] Compared with the prior art, the advantages and beneficial effects of the present invention are as follows: the coating prepared by the present invention has excellent anti-corrosion effect, and the coating is added with grafted modified graphene and modified fillers, so that the components of the coating are more compatible, a denser coating is formed, the adhesion is improved, the anti-corrosion effect is better, and it has broad application prospects. DETAILED DESCRIPTION
[0017] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] Example 1 This embodiment provides a method for preparing a heavy-duty anti-corrosion coating of grafted modified graphene, the preparation method comprising the following steps: (1) Under a nitrogen atmosphere, 1 part by mass of 3-isocyanate propyltrimethoxysilane and 0.14 parts by mass of graphene oxide were mixed, ultrasonicated for 22 min, 62 parts by mass of N,N-dimethylformamide were added, stirred at 103°C for 2.6 h, centrifuged, and the solid was freeze-dried to obtain isocyanate-modified graphene oxide; 10 parts by mass of isocyanate-modified filler were added to 62 parts by mass of ethanol, and then a 2.7 wt% aqueous solution of nano-cerium oxide was added dropwise; after the addition was completed, the mixture was stirred at 57°C for 2.4 h, centrifuged, and the solid was freeze-dried to obtain grafted modified graphene; (2) Add zinc powder into a three-necked flask, add toluene diisocyanate and isopropanol, add grafted modified graphene, and disperse them ultrasonically under nitrogen protection for 17 minutes. After dispersion, heat to 95°C, stir and react for 1.5 hours, filter, and dry the residue in a vacuum drying oven to obtain modified graphene-zinc composite powder; (3) According to the weight percentage, 36 parts of epoxy resin, 9 parts of modified filler, 12 parts of solvent, 1 part of leveling agent, 2 parts of dispersant, 0.3 parts of defoaming agent and 1.2 parts of silane coupling agent are selected respectively, mixed and added into a stirring tank in sequence, stirring is started, and the stirring speed is controlled to be 350r / min. 15 parts of modified graphene-zinc composite powder are added into the stirring tank in 4 times, stirring is continued for 22 minutes, and then added into a grinder for grinding, and the powder is ground to a particle size of less than 50μm, and the epoxy resin slurry is obtained, which is component A; (4) 12 parts by weight of isophorone diamine, 2 parts by weight of dibutyl phthalate and 8 parts by weight of n-butanol are mixed uniformly to obtain component B; (5) Component A and component B are packaged separately and mixed evenly at a mass ratio of 6:1 when used to obtain a heavy-duty anti-corrosion coating of grafted modified graphene.
[0019] The mass ratio of isocyanate-modified graphene oxide to nano-cerium oxide is 10:3.
[0020] The mass ratio of grafted modified graphene to zinc powder is 1:22.
[0021] The epoxy resin described in step (3) is bisphenol A type epoxy resin.
[0022] The solvent in step (3) is a mixture of butyl acetate and n-butanol in a mass ratio of 1:5.
[0023] The leveling agent in step (3) is leveling agent BYK-333; the defoaming agent is tributyl phosphate; and the silane coupling agent is KH-560.
[0024] The dispersant in step (3) is polyethylene wax.
[0025] The preparation method of the modified filler comprises the following steps: mixing filler, 55wt% ethanol aqueous solution and silane coupling agent KH550 in a mass ratio of 1:6:0.02, stirring and reacting at 60-65°C for 3h, filtering to obtain a solid, washing and drying to obtain the modified filler.
[0026] The filler comprises nano-aluminum oxide, nano-silicon nitride and nano-lanthanum oxide in a mass ratio of 1:1.4:0.6.
[0027] The particle size of nano-alumina is 200-300nm and the specific surface area is 40-55m 2 / g; the particle size of nano silicon nitride is 50-100nm, and the specific surface area is 30-43m 2 / g; the particle size of nano lanthanum oxide is 120-160nm, and the specific surface area is 15-35m 2 / g.
[0028] Comparative Example 1 The difference between this comparative example and Example 1 is that no grafted modified graphene is added.
[0029] A method for preparing a heavy-duty anticorrosive coating, the method comprising the following steps: (1) According to weight, 36 parts of epoxy resin, 9 parts of modified filler, 12 parts of solvent, 1 part of leveling agent, 2 parts of dispersant, 0.3 parts of defoamer and 1.2 parts of silane coupling agent are selected respectively, mixed and added to a stirring tank in sequence, stirring is started, and the stirring speed is controlled to 350r / min. 15 parts of zinc powder are added to the stirring tank in 4 times, and stirring is continued for 22 minutes. Then, the mixture is added to a grinder and ground until the particle size is less than 50μm. The epoxy resin slurry is obtained, which is component A; (2) 12 parts by weight of isophorone diamine, 2 parts by weight of dibutyl phthalate and 8 parts by weight of n-butanol, mixed evenly to obtain component B; (3) Package component A and component B separately and mix them evenly in a mass ratio of 6:1 to obtain a heavy-duty anti-corrosion coating.
[0030] The epoxy resin described in step (3) is bisphenol A type epoxy resin.
[0031] The solvent in step (3) is a mixture of butyl acetate and n-butanol in a mass ratio of 1:5.
[0032] The leveling agent in step (3) is leveling agent BYK-333; the defoaming agent is tributyl phosphate; and the silane coupling agent is KH-560.
[0033] The dispersant in step (3) is polyethylene wax.
[0034] The preparation method of the modified filler comprises the following steps: mixing filler, 55wt% ethanol aqueous solution and silane coupling agent KH550 in a mass ratio of 1:6:0.02, stirring and reacting at 60-65°C for 3h, filtering to obtain a solid, washing and drying to obtain the modified filler.
[0035] The filler comprises nano-aluminum oxide, nano-silicon nitride and nano-lanthanum oxide in a mass ratio of 1:1.4:0.6.
[0036] The particle size of nano-alumina is 200-300nm and the specific surface area is 40-55m 2 / g; the particle size of nano silicon nitride is 50-100nm, and the specific surface area is 30-43m 2 / g; the particle size of nano lanthanum oxide is 120-160nm, and the specific surface area is 15-35m 2 / g.
[0037] Comparative Example 2 The difference between this comparative example and Example 1 is that the grafted modified graphene is replaced by graphene oxide.
[0038] A method for preparing a heavy-duty anticorrosive coating, the method comprising the following steps: (1) Add zinc powder into a three-necked flask, add toluene diisocyanate and isopropanol, add graphene oxide, and ultrasonically disperse for 17 minutes under nitrogen protection. After dispersion, heat to 95°C, stir and react for 1.5 hours, filter, and dry the residue in a vacuum drying oven to obtain a modified graphene-zinc composite powder; (2) According to the weight percentage, 36 parts of epoxy resin, 9 parts of modified filler, 12 parts of solvent, 1 part of leveling agent, 2 parts of dispersant, 0.3 parts of defoaming agent and 1.2 parts of silane coupling agent are selected respectively, and the mixture is added into a stirring tank in sequence. Stirring is started and the stirring speed is controlled to be 350r / min. 15 parts of modified graphene-zinc composite powder are added into the stirring tank in 4 times. Stirring is continued for 22 minutes and then the powder is added into a grinder for grinding until the particle size is less than 50μm. The epoxy resin slurry is obtained as component A. (3) 12 parts by weight of isophorone diamine, 2 parts by weight of dibutyl phthalate and 8 parts by weight of n-butanol, mixed evenly to obtain component B; (4) Component A and component B are packaged separately and mixed evenly at a mass ratio of 6:1 when used to obtain a heavy-duty anti-corrosion coating of grafted modified graphene.
[0039] The mass ratio of graphene oxide to zinc powder is 1:22.
[0040] The epoxy resin described in step (3) is bisphenol A type epoxy resin.
[0041] The solvent in step (3) is a mixture of butyl acetate and n-butanol in a mass ratio of 1:5.
[0042] The leveling agent in step (3) is leveling agent BYK-333; the defoaming agent is tributyl phosphate; and the silane coupling agent is KH-560.
[0043] The dispersant in step (3) is polyethylene wax.
[0044] The preparation method of the modified filler comprises the following steps: mixing filler, 55wt% ethanol aqueous solution and silane coupling agent KH550 in a mass ratio of 1:6:0.02, stirring and reacting at 60-65°C for 3h, filtering to obtain a solid, washing and drying to obtain the modified filler.
[0045] The filler comprises nano-aluminum oxide, nano-silicon nitride and nano-lanthanum oxide in a mass ratio of 1:1.4:0.6.
[0046] The particle size of nano-alumina is 200-300nm and the specific surface area is 40-55m 2 / g; the particle size of nano silicon nitride is 50-100nm, and the specific surface area is 30-43m 2 / g; the particle size of nano lanthanum oxide is 120-160nm, and the specific surface area is 15-35m 2 / g.
[0047] Comparative Example 3 The difference between this comparative example and Example 1 is that the composition of the mixed filler is different.
[0048] A method for preparing a heavy-duty anti-corrosion coating of grafted modified graphene, the preparation method comprising the following steps: (1) Under a nitrogen atmosphere, 1 part by mass of 3-isocyanate propyltrimethoxysilane and 0.14 parts by mass of graphene oxide were mixed, ultrasonicated for 22 min, 62 parts by mass of N,N-dimethylformamide were added, stirred at 103°C for 2.6 h, centrifuged, and the solid was freeze-dried to obtain isocyanate-modified graphene oxide; 10 parts by mass of isocyanate-modified filler were added to 62 parts by mass of ethanol, and then a 2.7 wt% aqueous solution of nano-cerium oxide was added dropwise; after the addition was completed, the mixture was stirred at 57°C for 2.4 h, centrifuged, and the solid was freeze-dried to obtain grafted modified graphene; (2) Add zinc powder into a three-necked flask, add toluene diisocyanate and isopropanol, add grafted modified graphene, and disperse them ultrasonically under nitrogen protection for 17 minutes. After dispersion, heat to 95°C, stir and react for 1.5 hours, filter, and dry the residue in a vacuum drying oven to obtain modified graphene-zinc composite powder; (3) According to the weight percentage, 36 parts of epoxy resin, 9 parts of modified filler, 12 parts of solvent, 1 part of leveling agent, 2 parts of dispersant, 0.3 parts of defoaming agent and 1.2 parts of silane coupling agent are selected respectively, mixed and added into a stirring tank in sequence, stirring is started, and the stirring speed is controlled to be 350r / min. 15 parts of modified graphene-zinc composite powder are added into the stirring tank in 4 times, stirring is continued for 22 minutes, and then added into a grinder for grinding, and the powder is ground to a particle size of less than 50μm, and the epoxy resin slurry is obtained, which is component A; (4) 12 parts by weight of isophorone diamine, 2 parts by weight of dibutyl phthalate and 8 parts by weight of n-butanol are mixed uniformly to obtain component B; (5) Component A and component B are packaged separately and mixed evenly at a mass ratio of 6:1 when used to obtain a heavy-duty anti-corrosion coating of grafted modified graphene.
[0049] The mass ratio of isocyanate-modified graphene oxide to nano-cerium oxide is 10:3.
[0050] The mass ratio of grafted modified graphene to zinc powder is 1:22.
[0051] The epoxy resin described in step (3) is bisphenol A type epoxy resin.
[0052] The solvent in step (3) is a mixture of butyl acetate and n-butanol in a mass ratio of 1:5.
[0053] The leveling agent in step (3) is leveling agent BYK-333; the defoaming agent is tributyl phosphate; and the silane coupling agent is KH-560.
[0054] The dispersant in step (3) is polyethylene wax.
[0055] The preparation method of the modified filler comprises the following steps: mixing filler, 55wt% ethanol aqueous solution and silane coupling agent KH550 in a mass ratio of 1:6:0.02, stirring and reacting at 60-65°C for 3h, filtering to obtain a solid, washing and drying to obtain the modified filler.
[0056] The filler comprises nano-aluminum oxide, nano-silicon nitride and nano-lanthanum oxide in a mass ratio of 1:1:1.
[0057] The particle size of nano-alumina is 200-300nm and the specific surface area is 40-55m 2 / g; the particle size of nano silicon nitride is 50-100nm, and the specific surface area is 30-43m 2 / g; the particle size of nano lanthanum oxide is 120-160nm, and the specific surface area is 15-35m 2 / g. Comparative Example 4 The difference between this comparative example and Example 1 is that no modified filler is added.
[0058] A method for preparing a heavy-duty anti-corrosion coating of grafted modified graphene, the preparation method comprising the following steps: (1) Under a nitrogen atmosphere, 1 part by mass of 3-isocyanate propyltrimethoxysilane and 0.14 parts by mass of graphene oxide were mixed, ultrasonicated for 22 min, 62 parts by mass of N,N-dimethylformamide were added, stirred at 103°C for 2.6 h, centrifuged, and the solid was freeze-dried to obtain isocyanate-modified graphene oxide; 10 parts by mass of isocyanate-modified filler were added to 62 parts by mass of ethanol, and then a 2.7 wt% aqueous solution of nano-cerium oxide was added dropwise; after the addition was completed, the mixture was stirred at 57°C for 2.4 h, centrifuged, and the solid was freeze-dried to obtain grafted modified graphene; (2) Add zinc powder into a three-necked flask, add toluene diisocyanate and isopropanol, add grafted modified graphene, and disperse them ultrasonically under nitrogen protection for 17 minutes. After dispersion, heat to 95°C, stir and react for 1.5 hours, filter, and dry the residue in a vacuum drying oven to obtain modified graphene-zinc composite powder; (3) Select 36 parts of epoxy resin, 12 parts of solvent, 1 part of leveling agent, 2 parts of dispersant, 0.3 parts of defoaming agent and 1.2 parts of silane coupling agent by weight, mix them and add them to a stirring tank in sequence, start stirring, control the stirring speed to 350r / min, add 15 parts of modified graphene-zinc composite powder to the stirring tank in 4 times, continue stirring for 22 minutes, then add it to a grinder and grind it until the particle size is less than 50μm, and obtain epoxy resin slurry, which is component A; (4) 12 parts by weight of isophorone diamine, 2 parts by weight of dibutyl phthalate and 8 parts by weight of n-butanol are mixed uniformly to obtain component B; (5) Component A and component B are packaged separately and mixed evenly at a mass ratio of 6:1 when used to obtain a heavy-duty anti-corrosion coating of grafted modified graphene.
[0059] The mass ratio of isocyanate-modified graphene oxide to nano-cerium oxide is 10:3.
[0060] The mass ratio of grafted modified graphene to zinc powder is 1:22.
[0061] The epoxy resin described in step (3) is bisphenol A type epoxy resin.
[0062] The solvent in step (3) is a mixture of butyl acetate and n-butanol in a mass ratio of 1:5.
[0063] The leveling agent in step (3) is leveling agent BYK-333; the defoaming agent is tributyl phosphate; and the silane coupling agent is KH-560.
[0064] The dispersant in step (3) is polyethylene wax.
[0065] Comparative Example 5 The difference between this comparative example and Example 1 is that the modified filler is replaced by filler.
[0066] A method for preparing a heavy-duty anti-corrosion coating of grafted modified graphene, the preparation method comprising the following steps: (1) Under a nitrogen atmosphere, 1 part by mass of 3-isocyanate propyltrimethoxysilane and 0.14 parts by mass of graphene oxide were mixed, ultrasonicated for 22 min, 62 parts by mass of N,N-dimethylformamide were added, stirred at 103°C for 2.6 h, centrifuged, and the solid was freeze-dried to obtain isocyanate-modified graphene oxide; 10 parts by mass of isocyanate-modified filler were added to 62 parts by mass of ethanol, and then a 2.7 wt% aqueous solution of nano-cerium oxide was added dropwise; after the addition was completed, the mixture was stirred at 57°C for 2.4 h, centrifuged, and the solid was freeze-dried to obtain grafted modified graphene; (2) Add zinc powder into a three-necked flask, add toluene diisocyanate and isopropanol, add grafted modified graphene, and disperse them ultrasonically under nitrogen protection for 17 minutes. After dispersion, heat to 95°C, stir and react for 1.5 hours, filter, and dry the residue in a vacuum drying oven to obtain modified graphene-zinc composite powder; (3) According to the weight percentage, 36 parts of epoxy resin, 9 parts of filler, 12 parts of solvent, 1 part of leveling agent, 2 parts of dispersant, 0.3 parts of defoaming agent and 1.2 parts of silane coupling agent are selected respectively, mixed and added to a stirring tank in sequence, stirring is started, and the stirring speed is controlled to be 350r / min. 15 parts of modified graphene-zinc composite powder are added to the stirring tank in 4 times, and stirring is continued for 22 minutes. Then, the powder is added to a grinder and ground until the particle size is less than 50μm. The epoxy resin slurry is obtained, which is component A; (4) 12 parts by weight of isophorone diamine, 2 parts by weight of dibutyl phthalate and 8 parts by weight of n-butanol are mixed uniformly to obtain component B; (5) Component A and component B are packaged separately and mixed evenly at a mass ratio of 6:1 when used to obtain a heavy-duty anti-corrosion coating of grafted modified graphene.
[0067] The mass ratio of isocyanate-modified graphene oxide to nano-cerium oxide is 10:3.
[0068] The mass ratio of grafted modified graphene to zinc powder is 1:22.
[0069] The epoxy resin described in step (3) is bisphenol A type epoxy resin.
[0070] The solvent in step (3) is a mixture of butyl acetate and n-butanol in a mass ratio of 1:5.
[0071] The leveling agent in step (3) is leveling agent BYK-333; the defoaming agent is tributyl phosphate; and the silane coupling agent is KH-560.
[0072] The dispersant in step (3) is polyethylene wax.
[0073] The filler comprises nano-aluminum oxide, nano-silicon nitride and nano-lanthanum oxide in a mass ratio of 1:1.4:0.6.
[0074] The particle size of nano-alumina is 200-300nm and the specific surface area is 40-55m 2 / g; the particle size of nano silicon nitride is 50-100nm, and the specific surface area is 30-43m 2 / g; the particle size of nano lanthanum oxide is 120-160nm, and the specific surface area is 15-35m 2 / g.
[0075] Comparative Example 6 The difference between this comparative example and Example 1 is that the particle size of the filler is different.
[0076] A method for preparing a heavy-duty anti-corrosion coating of grafted modified graphene, the preparation method comprising the following steps: (1) Under a nitrogen atmosphere, 1 part by mass of 3-isocyanate propyltrimethoxysilane and 0.14 parts by mass of graphene oxide were mixed, ultrasonicated for 22 min, 62 parts by mass of N,N-dimethylformamide were added, stirred at 103°C for 2.6 h, centrifuged, and the solid was freeze-dried to obtain isocyanate-modified graphene oxide; 10 parts by mass of isocyanate-modified filler were added to 62 parts by mass of ethanol, and then a 2.7 wt% aqueous solution of nano-cerium oxide was added dropwise; after the addition was completed, the mixture was stirred at 57°C for 2.4 h, centrifuged, and the solid was freeze-dried to obtain grafted modified graphene; (2) Add zinc powder into a three-necked flask, add toluene diisocyanate and isopropanol, add grafted modified graphene, and disperse them ultrasonically under nitrogen protection for 17 minutes. After dispersion, heat to 95°C, stir and react for 1.5 hours, filter, and dry the residue in a vacuum drying oven to obtain modified graphene-zinc composite powder; (3) According to the weight percentage, 36 parts of epoxy resin, 9 parts of modified filler, 12 parts of solvent, 1 part of leveling agent, 2 parts of dispersant, 0.3 parts of defoaming agent and 1.2 parts of silane coupling agent are selected respectively, mixed and added into a stirring tank in sequence, stirring is started, and the stirring speed is controlled to be 350r / min. 15 parts of modified graphene-zinc composite powder are added into the stirring tank in 4 times, stirring is continued for 22 minutes, and then added into a grinder for grinding, and the powder is ground to a particle size of less than 50μm, and the epoxy resin slurry is obtained, which is component A; (4) 12 parts by weight of isophorone diamine, 2 parts by weight of dibutyl phthalate and 8 parts by weight of n-butanol are mixed uniformly to obtain component B; (5) Component A and component B are packaged separately and mixed evenly at a mass ratio of 6:1 when used to obtain a heavy-duty anti-corrosion coating of grafted modified graphene.
[0077] The mass ratio of isocyanate-modified graphene oxide to nano-cerium oxide is 10:3.
[0078] The mass ratio of grafted modified graphene to zinc powder is 1:22.
[0079] The epoxy resin described in step (3) is bisphenol A type epoxy resin.
[0080] The solvent in step (3) is a mixture of butyl acetate and n-butanol in a mass ratio of 1:5.
[0081] The leveling agent in step (3) is leveling agent BYK-333; the defoaming agent is tributyl phosphate; and the silane coupling agent is KH-560.
[0082] The dispersant in step (3) is polyethylene wax.
[0083] The preparation method of the modified filler comprises the following steps: mixing filler, 55wt% ethanol aqueous solution and silane coupling agent KH550 in a mass ratio of 1:6:0.02, stirring and reacting at 60-65°C for 3h, filtering to obtain a solid, washing and drying to obtain the modified filler.
[0084] The filler comprises nano-aluminum oxide, nano-silicon nitride and nano-lanthanum oxide in a mass ratio of 1:1.4:0.6.
[0085] The particle size of nano-alumina is 50-100nm and the specific surface area is 25-37m 2 / g; the particle size of nano silicon nitride is 250-300nm, and the specific surface area is 14-19m 2 / g; the particle size of nano lanthanum oxide is 350-370nm, and the specific surface area is 10-19m 2 / g.
[0086] Performance Testing The coatings of Example 1 and Comparative Examples 1-6 were used to prepare coatings, and the coatings were tested for performance. The test results are shown in Table 1.
[0087] Table 1 Performance test results
[0088] It can be seen from Table 1 that the coating of the present invention has an excellent anti-corrosion effect.
[0089] By comparing Example 1 with Comparative Examples 1-2, it can be seen that the grafted modified graphene described in the present invention can significantly improve the anti-corrosion effect.
[0090] By comparing Example 1 with Comparative Examples 3 to 6, it can be seen that the present invention significantly improves the anti-corrosion effect by modifying the filler, wherein the anti-corrosion effects of fillers with different ratios and parameters are different, and the modified filler obtained by modifying the filler ratio and parameters described in the present invention has a better anti-corrosion effect than that prepared by other types.
[0091] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a heavy-duty anti-corrosion coating of grafted modified graphene, characterized in that: The preparation method comprises the following steps: (1) Under a nitrogen atmosphere, 1 part by mass of 3-isocyanate propyl trimethoxy silane and 0.13-0.16 part by mass of graphene oxide are mixed, ultrasonicated for 20-25 min, 60-65 parts by mass of N, N-dimethylformamide are added, stirred at 102-105° C. for 2-3 h, centrifuged, and the solid is freeze-dried to obtain isocyanate-modified graphene oxide; 10 parts by mass of isocyanate-modified filler are added to 60-63 parts by mass of ethanol, and then a nano-cerium oxide aqueous solution with a mass percentage of 2.5-3.0wt% is added dropwise; after the addition is completed, stirring is continued at 56-58° C. for 2-3 h, centrifuged, and the solid is freeze-dried to obtain grafted modified graphene; (2) Add zinc powder to a three-necked flask, add toluene diisocyanate and isopropanol, add grafted modified graphene, and ultrasonically disperse for 15-20 minutes under nitrogen protection. After dispersion, heat to 90-100°C, stir and react for 1-2 hours, filter, and dry the residue in a vacuum drying oven to obtain modified graphene-zinc composite powder; (3) Select 34-38 parts of epoxy resin, 8-10 parts of modified filler, 10-15 parts of solvent, 1-2 parts of leveling agent, 1-2 parts of dispersant, 0.1-0.5 parts of defoaming agent and 1-1.3 parts of silane coupling agent by weight, mix them and add them to a stirring tank in sequence, start stirring, control the stirring speed to 300-400r / min, add 10-20 parts of modified graphene-zinc composite powder to the stirring tank in 3-5 times, continue stirring for 20-25 minutes, then add it to a grinder and grind it until the particle size is less than 50μm, and obtain epoxy resin slurry, which is component A; (4) 10-13 parts by weight of isophorone diamine, 2-3 parts by weight of dibutyl phthalate and 5-8 parts by weight of n-butanol, mixed evenly to obtain component B; (5) Component A and component B are packaged separately and mixed evenly at a mass ratio of 6-9:1 when used to obtain a heavy-duty anti-corrosion coating of grafted modified graphene.
2. The method for preparing the heavy-duty anticorrosion coating of grafted modified graphene according to claim 1, characterized in that: The mass ratio of isocyanate-modified graphene oxide to nano-cerium oxide is 10:(1-3).
3. The method for preparing the heavy-duty anticorrosion coating of grafted modified graphene according to claim 1, characterized in that: The mass ratio of grafted modified graphene to zinc powder is 1:20-23.
4. The method for preparing the heavy-duty anticorrosion coating of grafted modified graphene according to claim 1, characterized in that: The epoxy resin in step (3) is one of bisphenol A epoxy resin, novolac epoxy resin or silicone epoxy resin.
5. The method for preparing the heavy-duty anticorrosion coating of grafted modified graphene according to claim 1, characterized in that: The solvent in step (3) is a mixture of butyl acetate and n-butanol in a mass ratio of 1:
5.
6. The method for preparing the heavy-duty anticorrosion coating of grafted modified graphene according to claim 1, characterized in that: The leveling agent in step (3) is leveling agent BYK-333; the defoaming agent is one of tributyl phosphate or dimethyl silicone oil; and the silane coupling agent is KH-560.
7. The method for preparing the heavy-duty anticorrosion coating of grafted modified graphene according to claim 1, characterized in that: The dispersant in step (3) is one or more of polyethylene wax, polyvinyl pyrrolidone, sodium carboxymethyl cellulose, and polyethylene glycol.
8. The method for preparing the heavy-duty anticorrosion coating of grafted modified graphene according to claim 1, characterized in that: The preparation method of the modified filler comprises the following steps: mixing filler, 55wt% ethanol aqueous solution and silane coupling agent KH550 in a mass ratio of 1:6-8:0.02-0.03, stirring and reacting at 60-65°C for 2-4h, filtering to obtain a solid, washing and drying to obtain the modified filler.
9. The method for preparing the heavy-duty anticorrosion coating of grafted modified graphene according to claim 1, characterized in that: The filler comprises nano-aluminum oxide, nano-silicon nitride and nano-lanthanum oxide in a mass ratio of 1:1.3-1.5:0.5-0.
7.
10. The method for preparing the heavy-duty anti-corrosion coating of grafted modified graphene according to claim 1, characterized in that: The particle size of nano-alumina is 200-300nm and the specific surface area is 40-55m 2 / g; the particle size of nano silicon nitride is 50-100nm, and the specific surface area is 30-43m 2 / g; the particle size of nano lanthanum oxide is 120-160nm, and the specific surface area is 15-35m 2 / g.
Citation Information
Patent Citations
Ceramic coating material with characteristics of high-temperature resistance, high blackness, coking resistance and corrosion resistance
CN108299870A
Preparation method of epoxy zinc / graphene heavy-duty anticorrosive coating
CN109836964A
Amphiphilic graphene oxide and preparation method thereof and application in waterborne coating thereof
CN110240814A
Graphene modified anti-corrosion coating as well as preparation method and application thereof
CN115181478A
Doped layered cerium oxide and preparation method thereof
CN117414860A