High-temperature-resistant LDS functional coating and preparation method thereof

The high-temperature resistant LDS functional coating addresses the challenge of low precision and mechanical property loss in large parts by using a resin or ceramic matrix with LDS additives, enhancing surface roughness and precision in circuit manufacturing.

CN119081539AInactive Publication Date: 2024-12-06AVIC BEIJING AERONAUTICAL MFG TECH RES INST

Patent Information

Application Number
CN202411234592.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing LDS technologies face challenges in manufacturing high-precision circuits on large parts with high temperature resistance due to difficulties in mixing LDS additives with thermosetting resins, leading to low mechanical properties and surface roughness issues that affect circuit accuracy.

Method used

A high-temperature resistant LDS functional coating comprising a resin or ceramic matrix, solvent/dispersant, LDS additive, and auxiliary agents, with specific weight ratios, is developed to improve surface roughness and maintain mechanical properties, allowing for precise chemical plating on composite and ceramic materials.

Benefits of technology

The coating expands the LDS process's application to large parts with high temperature resistance, maintaining mechanical properties and achieving high precision in circuit manufacturing by improving surface roughness and preventing additive agglomeration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081539A_ABST
    Figure CN119081539A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of coatings, in particular to a high-temperature-resistant LDS functional coating and a preparation method thereof.The coating comprises a coating matrix, a solvent / dispersing agent, an LDS additive and auxiliaries, and the coating matrix is a resin matrix or a ceramic matrix; the coating comprises the following components in parts by weight: 30-98 parts of a coating matrix, 0-70 parts of a solvent / dispersant, 1-30 parts of an LDS additive and 0-30 parts of an auxiliary agent. The high-temperature-resistant LDS functional coating and the preparation method thereof aim at solving the problem that the precision of a circuit manufactured in a chemical plating process is low due to the fact that the surface roughness is large.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of surface engineering, and in particular to a high-temperature resistant LDS functional coating and a preparation method thereof. Background Art

[0002] LDS (Laser Direct Structuring) technology, also known as molded interconnect device (MID), is a process that directly transfers to the target part surface through laser processing, uses the three-dimensional surface of the three-dimensional part to form circuit interconnections, or realizes metallized vias through laser drilling. This traditional process evenly adds LDS activator to the part material, uses laser processing to scan the target pattern, laser activates and shallowly etches the part surface, and uses chemical plating to selectively deposit copper on the patterned part processed by laser to achieve the effect of patterned circuit preparation. In order to achieve the three-proof effect or to be suitable for special processes, other metal materials such as nickel, silver, and gold can also be deposited on the copper layer. The LDS process realizes the rapid manufacturing of three-dimensional circuits quickly, integratedly, and at low cost through simple laser scanning, and is widely used in communications, medical, automotive and other industries. At present, the traditional LDS material is to melt and evenly mix the LDS additive with the thermoplastic plastic to achieve the purpose of laser activation processing. LDS additives are mostly metal salts, which are added to the material body, greatly reducing the mechanical properties of the material. Due to the manufacturing process of thermosetting resins, LDS additives are difficult to mix and add. In addition, the LDS process is currently mainly used for small-sized parts with low requirements for mechanical properties of parts, such as mobile phones, smart watches, headphones, car speaker circuit boards, hearing aids and other consumer electronics parts. For large parts, adding LDS additives is expensive and the process is complicated.

[0003] At present, with the development of high performance materials, LDS additives cannot be added to the material itself. The target circuit manufacturing surface is mainly advanced composite materials and ceramics, which have high requirements for the temperature resistance of the surface coating. Affected by the target surface manufacturing process, the roughness is difficult to control or the control cost is high. The surface roughness needs to be improved for the chemical plating process to manufacture high-precision circuits.

[0004] Therefore, the inventor provides a high temperature resistant LDS functional coating and a preparation method thereof. Summary of the invention

[0005] (1) Technical issues to be solved

[0006] The embodiment of the present invention provides a high temperature resistant LDS functional coating and a preparation method thereof, which solves the technical problem of low precision of manufacturing circuits in a chemical plating process caused by large surface roughness.

[0007] (2) Technical solution

[0008] The first aspect of the present invention provides a high temperature resistant LDS functional coating, comprising a coating matrix, a solvent / dispersant, an LDS additive and an auxiliary agent, wherein the coating matrix is ​​a resin matrix or a ceramic matrix; the weight portion of the coating matrix is ​​30 to 98 parts, the weight portion of the solvent / dispersant is 0 to 70 parts, the weight portion of the LDS additive is 1 to 30 parts, and the weight portion of the auxiliary agent is 0 to 30 parts.

[0009] Furthermore, the resin matrix is ​​any one of a polymer, a monomer capable of generating a polymer, an oligomer and a prepolymer.

[0010] Furthermore, the resin matrix includes at least one of epoxy resin, bismaleimide resin, cyanate resin, polyimide resin, polyurethane, hydroxy polyether, urea-formaldehyde resin, polysiloxane, polysilazane, polysilane, polysilocarbonane, modified epoxy resin, phenolic resin, benzoxazine resin and melamine formaldehyde resin.

[0011] Furthermore, the resin matrix also includes at least one of polyethersulfoneketone, polyetheretherketone, polyaryletherketone, polyethersulfone, polysulfone, polyimide ether, polycarbonate, polyphenylene ether and liquid crystal polymer.

[0012] Furthermore, the ceramic matrix includes at least one of an inorganic-organic composite matrix composed of a metal oxide, a non-metal oxide, and an organic silicon resin.

[0013] Furthermore, the LDS additive is a metal salt of copper, arsenic or tin.

[0014] Furthermore, the LDS additive includes at least one of copper chromite, copper hydroxyphosphate, arsenic trioxide and tin dioxide.

[0015] Furthermore, the weight portion of the LDS additive is 3 to 10 parts.

[0016] The second aspect of the present invention provides a method for preparing the above-mentioned high temperature resistant LDS functional coating, comprising the following steps:

[0017] Weigh and prepare the resin matrix / ceramic matrix, solvent / dispersant, LDS additive and auxiliary agent according to a preset ratio;

[0018] After all components are configured, mix them thoroughly.

[0019] Furthermore, after the components are configured and fully mixed, the method further includes: adding a preset amount of solvent / dispersant again and fully mixing.

[0020] (3) Beneficial effects

[0021] In summary, the present invention expands the application scope and application scenarios of the LDS process (laser engraving-chemical plating) for preparing patterned conductive circuits by adding LDS additives to the coating. This material can be used to prepare metal circuits on the surface of composite materials, and the coating has high temperature resistance and can have the same service temperature as the composite material substrate. Since the LDS additive is not added to the base material, the base performance, especially the mechanical properties, dielectric properties, etc., will not be lost. At the same time, the LDS coating method improves the surface roughness of the substrate, and overcomes the problem of low circuit accuracy caused by the rough surface of the substrate in the chemical plating process. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments of the present invention are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0023] Figure 1 It is a schematic flow chart of a method for preparing a high temperature resistant LDS functional coating provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0024] The following detailed description of the embodiments of the present invention is provided in conjunction with the accompanying drawings and examples. The following detailed description of the embodiments and the accompanying drawings are used to illustrate the principles of the present invention, but cannot be used to limit the scope of the present invention, that is, the present invention is not limited to the described embodiments.

[0025] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0026] A high-temperature resistant LDS functional coating provided by an embodiment of the present invention includes a coating base, a solvent / dispersant, an LDS additive and an auxiliary agent, wherein the coating base is a resin base or a ceramic base; the weight portion of the coating base is 30 to 98 parts, the weight portion of the solvent / dispersant is 0 to 70 parts, the weight portion of the LDS additive is 1 to 30 parts, and the weight portion of the auxiliary agent is 0 to 30 parts.

[0027] In the above-mentioned embodiments, according to the different materials of the target parts, they can be roughly divided into organic thermosetting coatings and inorganic ceramic coatings. Organic thermosetting coatings are suitable for bonding with the surface of composite materials, and inorganic ceramic coatings are suitable for bonding with the surface of ceramics. The LDS process is extended to more materials, such as composite materials, ceramic materials, etc., which expands the application scope and application scenarios of the LDS process (laser engraving-chemical plating) for preparing patterned conductive circuits. Since the LDS additive is not added to the base material, the base performance will not be lost, especially the mechanical properties, dielectric properties and other aspects. At the same time, the LDS coating method improves the surface roughness of the substrate, and overcomes the problem of low circuit accuracy caused by the rough surface of the substrate in the chemical plating process. Among them, the coating base content affects the adhesion with the substrate, the solvent / dispersant content determines the viscosity of the finished coating, affects the construction performance, and the LDS additive content affects the plating of the metal circuit in the subsequent process and the precision and quality of the finished product. It is necessary to comprehensively consider the content of each component between the formulas and regulate the coating performance as a whole.

[0028] When LDS additives are added to the coating, due to the small particle size and light density of LDS additives, and the metal salt materials, they are prone to agglomeration, sedimentation, and uneven dispersion in the solvent. This will cause the coating to easily clog the nozzle during construction, and the filler in the paint layer after construction will be unevenly dispersed, which will ultimately affect the preparation and accuracy of the metal circuit. In order to ensure the uniformity of the dispersion of the key component LDS additive in the coating, it is necessary to add a certain amount of filler to promote the multi-phase fusion of the resin matrix, solvent / dispersant and LDS additive to prevent agglomeration and sedimentation.

[0029] Among them, the solvent or dispersant is mainly selected according to the resin or ceramic matrix system, and can be water, aliphatic hydrocarbons, alicyclic hydrocarbons, such as naphtha, solvent oil; rosin water aromatic hydrocarbons, such as toluene, xylene and high flash point aromatic oil; ketones, esters, such as methyl ethyl ketone (MEK), methyl isobutyl ketone, isophorone, propylene glycol methyl ether acetate, ether acetate, butanone, acetone, cyclohexanone; ethers such as ethylene glycol ethyl ether, ethylene glycol monobutyl ether, propylene glycol propyl ether, ethylene glycol monobutyl ether; alcohols, such as methanol, ethanol, isopropanol, n-butanol, sec-butanol, isobutanol, isooctyl alcohol, cyclohexanol, etc.

[0030] LDS additives are used to activate the reaction during the laser engraving process, thereby achieving selective chemical plating (chemical deposition). They are usually metal salts of copper or tin, such as copper chromite (copper chrome black), copper hydroxyphosphate (basic copper phosphate), arsenic trioxide, tin dioxide, etc.

[0031] The additives can be leveling agents, defoamers, drying agents, anti-skinning agents, anti-settling agents, antioxidants, mildew inhibitors, curing agents, accelerators, plasticizers, slow-release agents, rust removers, foaming agents, photosensitizers, tackifiers, coupling agents. The additives here can also be powders, particles, microbeads, fibers added to improve the performance of the coating, such as continuous or chopped fibers, organic fibers, inorganic fibers or metal wires, including carbon fibers, glass fibers, quartz fibers, mullite fibers, basalt fibers, lignin fibers, natural fibers, carbon nanotube fibers, ceramic fibers, boron fibers, aramid fibers, Kevlar fibers, ultra-high molecular weight polyethylene fibers, liquid crystal polymers (LCP), optical fibers, polyaryletherketone fibers, nylon fibers, polyimide fibers , such as polymer powder, polytetrafluoroethylene powder, liquid crystal polymer powder, glass beads, ceramic beads, carbon nanotubes, graphene, alumina (corundum), zinc oxide, titanium dioxide, mullite, calcium carbonate, magnesium carbonate, calcium silicate, aluminum silicate, magnesium silicate, potassium aluminum silicate, barium sulfate, silicon carbide, silicon nitride, boron nitride, silicon dioxide, whiskers, zirconium dioxide, yttrium dioxide, tungsten sulfide, adamantane, montmorillonite, nanosilver, cage-type polyhedral oligomeric silsesquioxane (POSS), MXene, ferrite, toner, etc.

[0032] Due to the high viscosity of high temperature resistant coatings, it is necessary to add certain additives to improve the coating's workability. Since laser processing is required on the coating surface later, in order to ensure processing accuracy, it is necessary to add certain additives to improve the hardness and mechanical properties of the coating after curing.

[0033] As an optional embodiment, the resin matrix is ​​any one of a polymer, a monomer that can generate a polymer, an oligomer and a prepolymer. Further, a suitable resin matrix is ​​selected according to the surface of the adapted part, such as an organosilicon resin, an organic fluorine coating, an organic titanium coating, a polysiloxane, a polysiloxane, a polysilazane, a polysilane, and a polysilocarbon. The resin matrix includes at least one of epoxy resin, bismaleimide resin, cyanate resin, polyimide resin, polyurethane, hydroxy polyether, urea-formaldehyde resin, polysiloxane, polysilazane, polysilane, polysilocarbon, modified epoxy resin, phenolic resin, benzoxazine resin and melamine formaldehyde resin. The resin matrix also includes at least one of polyether sulfone ketone, polyether ether ketone, polyarylether ketone, polyether sulfone, polysulfone, polyimide ether, polycarbonate, polyphenylene ether and liquid crystal polymer. The high temperature resistant resin matrix usually has an aromatic or silicone-containing molecular structure, which usually exhibits high viscosity, high molecular polarity, and poor compatibility with solvents / dispersants, which is specifically manifested in poor coating construction properties.

[0034] It should be noted here that the selection of the resin matrix is ​​determined according to the subsequent processing steps of the substrate and the type of substrate. The subsequent processing steps of the substrate refer to whether the surface needs to be further encapsulated, whether the substrate needs to be sprayed with other materials again, whether the substrate needs to be further bonded, etc. after the LDS process manufacturing line. The type of substrate refers to the service environment of the substrate, the adhesion between the substrate and the coating, etc. For composite material substrates, the same resin matrix is ​​preferably used as the coating resin matrix to improve the adhesion between the coating and the substrate. For example, for bismaleimide resin prepreg composite material substrates, it is suitable for coating matrices with bismaleimide monomer (BMI) and its oligomer prepolymer as the main component. In order to ensure the toughness of the coating, toughening agents or toughening curing agents are often added to the bismaleimide resin material. Diamines, bisphenols, epoxy, thermoplastic resins and other materials are often selected to improve the performance of the coating resin matrix. The composite material substrate prepared from cyanate resin prepreg is suitable for coating matrix with cyanate resin and its oligomer prepolymer as the main component. Depending on the application scenarios of the coating, different types of cyanate resins can be selected to adjust the heat resistance, glass transition temperature, dielectric constant, dielectric loss and other properties. Preferably, the cyanate resin is bisphenol A cyanate monomer, bisphenol A cyanate prepolymer, dicyclopentadiene cyanate, dicyclopentadiene cyanate prepolymer, phenolic cyanate monomer, phenolic cyanate monomer, etc. For thermoplastic composite material substrates, such as polyetheretherketone composite materials, polyaryletherketone composite materials, polyetherimide composite materials, polyphenylene sulfide composite materials, polyarylate composite materials, polyimide composite materials, liquid crystal elastomer composite materials, polyethersulfone composite materials, polyethersulfoneketone composite materials, etc., one or more of organic silicone resin, polyimide resin, phenolic resin and other resins are often used as the coating matrix.

[0035] As an optional embodiment, the ceramic matrix includes at least one of an inorganic-organic composite matrix composed of a metal oxide, a non-metallic oxide, and an organic silicon resin. Specifically, the ceramic matrix is ​​mainly an inorganic-organic composite matrix composed of a metal oxide or a non-metallic oxide or a small amount of an organic silicon resin, such as a hydrolyzate or hydrolyzate oligomer of elements such as silicon, aluminum, titanium, zirconium, molybdenum, cerium, and iridium, including ethyl silicate, silicate, silica sol, or silicon, aluminum, titanium, zirconium, molybdenum, cerium, iridium, and other element oxide powder materials. It should be noted that for ceramic substrates, the same material or the same element ceramic is often used as a coating substrate. In order to regulate adhesion, silicone resins, epoxy resins, etc. are often compounded therein.

[0036] As an optional embodiment, the LDS additive is a metal salt of copper, arsenic or tin. The LDS additive includes at least one of copper chromite, copper hydroxyphosphate, arsenic trioxide and tin dioxide.

[0037] Furthermore, the weight portion of the LDS additive is 3 to 10 parts.

[0038] Figure 1 is a schematic diagram of a method for preparing a high temperature resistant LDS functional coating provided by an embodiment of the present invention, such as Figure 1 As shown, the method may include the following steps:

[0039] S100, weighing and preparing the resin matrix / ceramic matrix, solvent / dispersant, LDS additive and auxiliary agent according to a preset ratio.

[0040] S200, after all components are configured, mix them thoroughly and evenly.

[0041] As an optional implementation, after the components are configured and fully mixed in step S200, the process further includes: adding a preset amount of solvent / dispersant again and fully mixing. Specifically, for resin coatings, the resin needs to be allowed to stand for a long time to dissolve, and then mixed again.

[0042] Example 1

[0043] The method for preparing a high temperature resistant LDS functional coating comprises the following steps:

[0044] (1) Take 30-70 parts of bismaleimide prepolymer, 1-30 parts of diamine curing agent or diallyl bisphenol A or epoxy resin (such as E-51, E-44, F-51, AG-80, etc.), 0.1 parts of leveling agent, 0.1 parts of defoaming agent, 5-50 parts of cyclohexanone solvent, and 5 parts of copper chromite in a container, add a stirring paddle and stir thoroughly for 30 minutes;

[0045] (2) Let stand for 2 hours until the resin is fully dissolved;

[0046] (3) The mixed liquid was transferred to a planetary ball mill and operated for 2 hours.

[0047] Example 2

[0048] The method for preparing a high temperature resistant LDS functional coating comprises the following steps:

[0049] (1) 50-80 parts of bisphenol A cyanate prepolymer, 20-50 parts of butanone solvent, 0.1 parts of leveling agent, 0.1 parts of defoaming agent, 0.5 parts of drying agent, and 10 parts of hydroxy copper phosphate are placed in a container, and a stirring paddle is added to fully stir for 30 minutes;

[0050] (2) Let stand for 24 hours until the resin is fully dissolved;

[0051] (3) Add a stirring paddle and stir thoroughly for 3 hours.

[0052] Example 3

[0053] The method for preparing a high temperature resistant LDS functional coating comprises the following steps:

[0054] Take 80-90 parts of epoxy resin emulsion, 0-10 parts of glass powder, 0.5 parts of leveling agent, 0.3 parts of defoaming agent and 10 parts of hydroxy copper phosphate in a container, add a stirring paddle and stir thoroughly for 3 hours.

[0055] It should be clear that the various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. The present invention is not limited to the specific steps and structures described above and shown in the figures. In addition, for the sake of brevity, a detailed description of known methods and technologies is omitted here.

[0056] The above are only embodiments of the present application and are not limited to the present application. For those skilled in the art, the present application may have various changes and variations without departing from the scope of the present invention. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.

Claims

1. A high temperature resistant LDS functional coating, characterized in that: The invention comprises a coating matrix, a solvent / dispersant, an LDS additive and an auxiliary agent, wherein the coating matrix is ​​a resin matrix or a ceramic matrix; the weight portion of the coating matrix is ​​30 to 98 parts, the weight portion of the solvent / dispersant is 0 to 70 parts, the weight portion of the LDS additive is 1 to 30 parts, and the weight portion of the auxiliary agent is 0 to 30 parts.

2. The high temperature resistant LDS functional coating according to claim 1, characterized in that: The resin matrix is ​​any one of a polymer, a monomer capable of generating a polymer, an oligomer and a prepolymer.

3. The high temperature resistant LDS functional coating according to claim 1 or 2, characterized in that: The resin matrix includes at least one of epoxy resin, bismaleimide resin, cyanate resin, polyimide resin, polyurethane, hydroxy polyether, urea-formaldehyde resin, polysiloxane, polysilazane, polysilane, polysilocarbonane, modified epoxy resin, phenolic resin, benzoxazine resin and melamine formaldehyde resin.

4. The high temperature resistant LDS functional coating according to claim 1, characterized in that: The resin matrix also includes at least one of polyethersulfoneketone, polyetheretherketone, polyaryletherketone, polyethersulfone, polysulfone, polyimide ether, polycarbonate, polyphenylene ether and liquid crystal polymer.

5. The high temperature resistant LDS functional coating according to claim 1, characterized in that: The ceramic matrix includes at least one of an inorganic-organic composite matrix composed of a metal oxide, a non-metal oxide, and an organic silicon resin.

6. The high temperature resistant LDS functional coating according to claim 1, characterized in that: The LDS additive is a metal salt of copper, arsenic or tin.

7. The high temperature resistant LDS functional coating according to claim 6, characterized in that: The LDS additive includes at least one of copper chromite, copper hydroxyphosphate, arsenic trioxide and tin dioxide.

8. The high temperature resistant LDS functional coating according to claim 1, characterized in that: The weight portion of the LDS additive is 3 to 10 parts.

9. A method for preparing a high temperature resistant LDS functional coating as claimed in any one of claims 1 to 8, characterized in that: The method comprises the following steps: Weigh and prepare the resin matrix / ceramic matrix, solvent / dispersant, LDS additive and auxiliary agent according to a preset ratio; After all components are configured, mix them thoroughly.

10. The preparation method according to claim 9, characterized in that: After the components are configured and fully mixed, the method further comprises: Add the preset amount of solvent / dispersant again and mix thoroughly.

Citation Information

Patent Citations

  • Core-shell composite inorganic metal oxides and method of preparation for prevention of thermal oxidative degradation in polymer and resin compositions

    CN106574105A

  • Powder spraying material with laser directly structuring function and preparation and applications thereof

    CN108822602A

  • High-temperature coating material for forming weldable metal circuit, and preparation method thereof

    CN110982374A

  • Liquid composition, and method for producing film and laminate using said liquid composition

    CN113817366A

  • Coating for three-dimensional structure integrated circuit and preparation method thereof

    CN115612333A

Cited By

  • Surface wear-resistant cable and preparation method thereof

    CN120748821A