High-temperature-resistant single-component water-based paint and preparation method thereof
By using modified mica powder and epoxy modified silicone resin in water-based coatings, combined with specific modifiers, the existing high-temperature water-based coatings need to be baked at high temperature and have low adhesion, and the need to bake without baking High-temperature resistant water-based coating with strong dry and adhesion meets the protection needs of steel plates.
Patent Information
- Application Number
- CN202411395587.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-12-06
AI Technical Summary
Existing high-temperature resistant water-based coatings require high-temperature baking to dry, and have low adhesion and flexibility, making it difficult to achieve good protection on steel plates.
Using a one-component aqueous coating formulation, including epoxy modified silicone resin, modified mica powder and specific modifiers, through dimethylbisoctadecyl ammonium chloride and 6-hydroxyethylsulfone-2- Naphthylamine modifies mica powder, combines suitable mass ratios and preparation methods to improve the high temperature resistance and adhesion of the coating.
It realizes a self-drying coating without high temperature baking, with high hardness and strong adhesion, and can keep it off in an environment of 500℃, which significantly improves the high temperature resistance and adhesion of water-based coatings.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of coatings, and in particular to a high temperature resistant single-component water-based coating and a preparation method thereof. Background Art
[0002] In today's coatings industry, water-based coatings are gradually becoming a focus of attention. With the increasing awareness of environmental protection and the urgent need for sustainable development, traditional solvent-based coatings are facing more and more challenges because they contain a large amount of volatile organic compounds. Therefore, as a low-carbon, environmentally friendly alternative, the market demand for water-based coatings has grown accordingly. However, in many industrial production processes, equipment and components are often in high-temperature environments, which requires water-based coatings to have good high-temperature resistance to protect metal surfaces from corrosion, oxidation and other damage. Most of the existing high-temperature resistant coatings are two-component coatings that need to be baked at a high temperature of more than 200°C to dry, which affects construction, and ordinary high-temperature paints have high hardness and poor adhesion and flexibility. Therefore, it is urgent to develop a high-temperature resistant water-based coating that is easy to apply and has strong adhesion and flexibility on steel plates. Summary of the invention
[0003] The present invention provides a high temperature resistant single-component water-based paint and a preparation method thereof, which can dry by itself without high temperature baking and is easy to construct, thus solving the problems in the related art that water-based paint needs high temperature baking and drying and has low flexibility and adhesion.
[0004] The technical solution of the present invention is as follows: The present invention provides a high temperature resistant single-component water-based paint, comprising the following raw materials in parts by weight: 50-60 parts of epoxy modified silicone resin, 0.5-0.7 parts of defoaming agent, 1-2 parts of dispersant, 5-10 parts of pigment, 24-30 parts of functional filler, and 10-20 parts of water; the functional filler is obtained by modifying mica powder with a modifier, and the modifier includes dimethyl dioctadecyl ammonium chloride.
[0005] As a further technical solution, the amount of the modifier added is 5% to 10% of the mass of the mica powder.
[0006] As a further technical solution, the modifier also includes 6-hydroxyethylsulfone-2-naphthylamine.
[0007] In the present invention, the mica powder is modified by dimethyl dioctadecyl ammonium chloride and 6-hydroxyethyl sulfone-2-naphthylamine, so that the high temperature resistance and adhesion of the water-based coating are further improved.
[0008] As a further technical solution, the mass ratio of the dimethyl dioctadecyl ammonium chloride to 6-hydroxyethyl sulfone-2-naphthylamine is 2-4:1.
[0009] In the present invention, by limiting the mass ratio of dimethyl dioctadecyl ammonium chloride to 6-hydroxyethyl sulfone-2-naphthylamine to 2-4:1, the high temperature resistance and adhesion of the water-based coating can be further improved.
[0010] As a further technical solution, the mass ratio of the dimethyldioctadecylammonium chloride to 6-hydroxyethylsulfone-2-naphthylamine is 3:1.
[0011] As a further technical solution, the method for preparing the functional filler comprises the following steps: adding mica powder into methanol, adding a modifier for modification, and obtaining the functional filler through drying.
[0012] As a further technical solution, the modification temperature is 50-60°C and the modification time is 7-9h.
[0013] As a further technical solution, the epoxy-modified silicone resin includes a first epoxy-modified silicone resin and a second epoxy-modified silicone resin, and the first epoxy-modified silicone resin and the second epoxy-modified silicone resin have different silicone ratios.
[0014] As a further technical solution, the silicone ratio of the first epoxy-modified silicone resin is 15% to 30%, and the silicone ratio of the second epoxy-modified silicone resin is 50% to 90%.
[0015] As a further technical solution, the mass ratio of the first epoxy-modified silicone resin to the second epoxy-modified silicone resin is 1:5-9.
[0016] In the present invention, by limiting the mass ratio of the first epoxy-modified silicone resin to the second epoxy-modified silicone resin to 1:5-9, the high temperature resistance and adhesion of the water-based coating are further improved.
[0017] As a further technical solution, the mass ratio of the first epoxy-modified silicone resin to the second epoxy-modified silicone resin is 1:7.
[0018] As a further technical solution, the dispersant includes one or more of alkyl polyoxyethylene ether, ethyl acetate, and hydroxypropyl methylcellulose.
[0019] As a further technical solution, the defoaming agent includes one or two of polydimethylsiloxane and polyoxypropylene glycerol ether.
[0020] The present invention also provides a method for preparing a high temperature resistant single-component water-based coating, comprising the following steps: mixing the raw materials uniformly to obtain the high temperature resistant single-component water-based coating.
[0021] The working principle and beneficial effects of the present invention are: 1. Existing high temperature resistant water-based coatings are usually two-component and require high temperature baking to dry, and the construction is unchanged. The high temperature resistant water-based coating of the present invention is a single component and does not require baking, and can be self-dried. It has a fast drying time, is easy to construct and saves energy, and has high hardness and good adhesion, and the hardness can reach 5H.
[0022] 2. In the present invention, the excellent heat resistance of the silicone resin in the epoxy-modified silicone resin can maintain stable physical and chemical properties at higher temperatures. The introduction of the epoxy resin improves the mechanical properties of the silicone resin, making it have higher strength and toughness. Therefore, adding the epoxy-modified silicone resin to the water-based coating can improve the high temperature resistance and adhesion of the water-based coating. Adding the functional filler of mica powder modified by dimethyl dioctadecyl ammonium chloride to the water-based coating further improves the high temperature resistance and adhesion of the water-based coating, solving the problem of poor high temperature resistance and low adhesion of the water-based coating. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] In the following embodiments and comparative examples: Mica powder, particle size 200 mesh; alkyl polyoxyethylene ether, model: Laureth-15; polydimethylsiloxane, CAS: 9016-00-6, purchased from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd.; polyoxypropylene glycerol ether, hydroxyl value: 45~56mg / g; hydroxypropyl methylcellulose, model: HPMC, purchased from Zhengzhou Xinqishun Chemical Products Co., Ltd.; epoxy modified silicone resin, model: DC-805, silicone ratio: 50%~90%; model: DC-840, silicone ratio: 15%~30%.
[0025] Example 1 A method for preparing a high temperature resistant one-component water-based coating comprises the following steps: 50 parts of DC-840 epoxy-modified silicone resin, 0.5 parts of polydimethylsiloxane, 1 part of alkyl polyoxyethylene ether, 5 parts of pigment, 24 parts of functional filler and 10 parts of water were uniformly stirred to obtain a single-component water-based coating.
[0026] The method for preparing a functional filler comprises the following steps: 60 g of mica powder (200 mesh) was added to 500 mL of methanol solution and mixed evenly, and then 3 g of dimethyl dioctadecyl ammonium chloride was added. The temperature was raised to 50° C., stirred for 9 hours, and dried to obtain a functional filler.
[0027] Example 2 A method for preparing a high temperature resistant one-component water-based coating comprises the following steps: 55 parts of DC-840 epoxy-modified silicone resin, 0.6 parts of polyoxypropylene glycerol ether, 1 part of ethyl acetate, 7 parts of pigment, 27 parts of functional filler and 15 parts of water were uniformly stirred to obtain a single-component water-based coating.
[0028] The method for preparing a functional filler comprises the following steps: 60 g of mica powder (200 mesh) was added to 500 mL of methanol solution and mixed evenly, and then 4.2 g of dimethyl dioctadecyl ammonium chloride was added. The temperature was raised to 55° C., stirred for 8 h, and dried to obtain a functional filler.
[0029] Example 3 A method for preparing a high temperature resistant one-component water-based coating comprises the following steps: 60 parts of DC-840 epoxy-modified silicone resin, 0.7 parts of polyoxypropylene glycerol ether, 2 parts of hydroxypropyl methylcellulose, 10 parts of pigment, 30 parts of functional filler and 20 parts of water were uniformly stirred to obtain a single-component water-based coating.
[0030] The method for preparing a functional filler comprises the following steps: 60 g of mica powder (200 mesh) was added to 500 mL of methanol solution and mixed evenly, and then 6 g of dimethyl dioctadecyl ammonium chloride was added. The temperature was raised to 60° C., stirred for 7 hours, and dried to obtain a functional filler.
[0031] Example 4 The present embodiment is different from the embodiment 1 only in that the preparation method of the functional filler comprises the following steps: adding 60 g of mica powder to 500 mL of methanol solution and mixing evenly, adding 1.5 g of dimethyldioctadecylammonium chloride and 1.5 g of 6-hydroxyethylsulfone-2-naphthylamine, heating to 50° C., stirring for 9 h, and drying to obtain the functional filler.
[0032] Example 5 The difference between this embodiment and embodiment 4 is that the addition amount of dimethyldioctadecylammonium chloride is 2.5 g, and the addition amount of 6-hydroxyethylsulfonyl-2-naphthylamine is 0.5 g.
[0033] Example 6 The difference between this embodiment and embodiment 4 is that the addition amount of dimethyldioctadecylammonium chloride is 2 g, and the addition amount of 6-hydroxyethylsulfonyl-2-naphthylamine is 1 g.
[0034] Example 7 The difference between this embodiment and embodiment 4 is that the addition amount of dimethyldioctadecylammonium chloride is 2.25 g, and the addition amount of 6-hydroxyethylsulfonyl-2-naphthylamine is 0.75 g.
[0035] Example 8 The difference between this embodiment and embodiment 4 is that the addition amount of dimethyldioctadecylammonium chloride is 2.4 g, and the addition amount of 6-hydroxyethylsulfonyl-2-naphthylamine is 0.6 g.
[0036] Example 9 The only difference between this embodiment and embodiment 7 is that the DC-840 epoxy-modified silicone resin is replaced by an equal amount of DC-805 epoxy-modified silicone resin.
[0037] Example 10 The only difference between this embodiment and embodiment 7 is that the DC-840 epoxy-modified silicone resin is replaced by an equal amount of DC-805 epoxy-modified silicone resin at a mass ratio of 1:2.
[0038] Embodiment 11 The only difference between this embodiment and embodiment 7 is that the DC-840 epoxy-modified silicone resin is replaced by an equal amount of DC-805 epoxy-modified silicone resin at a mass ratio of 1:10.
[0039] Example 12 The only difference between this embodiment and embodiment 7 is that the DC-840 epoxy-modified silicone resin is replaced by an equal amount of DC-805 epoxy-modified silicone resin at a mass ratio of 1:5.
[0040] Embodiment 13 The only difference between this embodiment and embodiment 7 is that the DC-840 epoxy-modified silicone resin is replaced by an equal amount of DC-805 epoxy-modified silicone resin at a mass ratio of 1:7.
[0041] Embodiment 14 The only difference between this embodiment and embodiment 7 is that the DC-840 epoxy-modified silicone resin is replaced by an equal amount of DC-805 epoxy-modified silicone resin at a mass ratio of 1:9.
[0042] Comparative Example 1 The only difference between this comparative example and Example 1 is that the functional filler is replaced by an equal amount of mica powder (200 mesh).
[0043] The single-component water-based coatings prepared in Examples 1 to 14 and Comparative Example 1 were tested for high temperature resistance and adhesion, and the test methods are as follows: High temperature resistance: Tested according to the test method in GB / T 1735-2009 "Determination of heat resistance of paints and varnishes", with a coating thickness of 400μm, a steel plate as the substrate, and a heating temperature of 500℃, to determine the longest time the coating remains free of peeling and cracking; Adhesion: The test was carried out according to the measurement method in GB / T 9286-2021 "Scratch test for paints and varnishes", with a coating thickness of 400μm and a substrate of steel plate. The test results are shown in Table 1.
[0044] Table 1 Single-component waterborne coating performance test results
[0045] Compared with Example 1, the mica powder was not modified in Example 1. As a result, the high temperature resistance time of the water-based coating prepared in Example 1 was lower than that in Example 1, indicating that modifying the mica powder with dimethyl dioctadecyl ammonium chloride can improve the high temperature resistance of the water-based coating.
[0046] Compared with Example 1, in Example 4, dimethyldioctadecylammonium chloride and 6-hydroxyethylsulfonyl-2-naphthylamine are used to modify the mica powder at the same time, and the mass ratio of dimethyldioctadecylammonium chloride and 6-hydroxyethylsulfonyl-2-naphthylamine is changed in Examples 5 to 8. As a result, the high temperature resistant time and adhesion of the water-based coatings in Examples 4 to 8 are higher than those in Example 1, and the high temperature resistant time of the water-based coatings in Examples 6 to 8 is higher than that in Examples 4 and 5, indicating that when the mass ratio of dimethyldioctadecylammonium chloride and 6-hydroxyethylsulfonyl-2-naphthylamine is 2 to 4:1, the high temperature resistance of the water-based coating can be further improved; comparing Examples 6 to 8, the high temperature resistant time of the water-based coating in Example 7 is higher than that in Examples 6 and 8, indicating that when the mass ratio of dimethyldioctadecylammonium chloride and 6-hydroxyethylsulfonyl-2-naphthylamine is 3:1, the obtained water-based coating has the best high temperature resistance.
[0047] Compared with Example 7, in Example 9, the DC-840 epoxy-modified silicone resin is replaced by the DC-805 epoxy-modified silicone resin, and in Examples 10 to 14, the epoxy-modified silicone resin is composed of the DC-840 epoxy-modified silicone resin and the DC-805 epoxy-modified silicone resin. As a result, the high temperature resistance time and adhesion of the water-based coatings prepared in Examples 9 to 11 are higher than those in Example 1, indicating that the epoxy-modified silicone resin is composed of the DC-840 epoxy-modified silicone resin and the DC-805 epoxy-modified silicone resin, which can improve the high temperature resistance time and adhesion of the water-based coating; Comparative Example 1 0~14, it is found that the high temperature resistance time and adhesion of the water-based coating in Examples 12~14 are higher than those in Examples 10 and 11, indicating that when the mass ratio of DC-840 epoxy-modified silicone resin to DC-805 epoxy-modified silicone resin is 1:5~9, the high temperature resistance time and adhesion of the water-based coating can be further improved; by comparing Examples 12~14, it is found that the high temperature resistance time of the water-based coating in Example 13 is higher than that in Examples 12 and 14, indicating that when the mass ratio of DC-840 epoxy-modified silicone resin to DC-805 epoxy-modified silicone resin is 1:7, the obtained water-based coating has the best high temperature resistance.
[0048] The high temperature resistant one-component water-based coatings prepared in Examples 1 to 14 of the present invention do not require high temperature baking and can dry themselves at room temperature. After testing, at 25° C., the surface drying time is ≤2h, the actual drying time is ≤24h, the drying time is short, and the construction is convenient.
[0049] The high temperature resistant one-component water-based coatings prepared in Examples 1 to 14 of the present invention have a flat and smooth appearance, a viscosity (No. 4 cup) ≥ 60, a glossiness (60°) of 10 to 30, and a heat resistance (500°C, 24h) coating that does not fall off or crack, meeting the technical requirements of water-based high temperature resistant topcoats.
[0050] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high temperature resistant one-component water-based coating, characterized in that: The raw materials include the following components in parts by weight: 50-60 parts of epoxy-modified silicone resin, 0.5-0.7 parts of defoaming agent, 1-2 parts of dispersant, 5-10 parts of pigment, 24-30 parts of functional filler and 10-20 parts of water; the functional filler is mica powder modified by a modifier, and the modifier includes dimethyl dioctadecyl ammonium chloride.
2. A high temperature resistant one-component water-based paint according to claim 1, characterized in that: The amount of the modifier added is 5% to 10% of the mass of the mica powder.
3. A high temperature resistant one-component water-based paint according to claim 1, characterized in that: The modifier also includes 6-hydroxyethylsulfonyl-2-naphthylamine.
4. A high temperature resistant one-component water-based paint according to claim 3, characterized in that: The mass ratio of the dimethyl dioctadecyl ammonium chloride to 6-hydroxyethyl sulfone-2-naphthylamine is 2-4:
1.
5. The high temperature resistant one-component water-based paint according to claim 1, characterized in that: The epoxy-modified silicone resin includes a first epoxy-modified silicone resin and a second epoxy-modified silicone resin, and the first epoxy-modified silicone resin and the second epoxy-modified silicone resin have different silicone ratios.
6. A high temperature resistant one-component water-based paint according to claim 5, characterized in that: The organic silicon ratio of the first epoxy-modified organic silicon resin is 15% to 30%, and the organic silicon ratio of the second epoxy-modified organic silicon resin is 50% to 90%.
7. The high temperature resistant one-component water-based paint according to claim 5, characterized in that: The mass ratio of the first epoxy-modified silicone resin to the second epoxy-modified silicone resin is 1:5-9.
8. The high temperature resistant one-component water-based paint according to claim 1, characterized in that: The dispersant includes one or more of alkyl polyoxyethylene ether, ethyl acetate, and hydroxypropyl methylcellulose.
9. The high temperature resistant one-component water-based paint according to claim 1, characterized in that: The defoaming agent includes one or two of polydimethylsiloxane and polyoxypropylene glycerol ether.
10. The method for preparing a high temperature resistant one-component water-based coating according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: the raw materials are mixed evenly to obtain a high temperature resistant single-component water-based coating.
Citation Information
Patent Citations
Water-based high-temperature-resistant paint
CN110484131A
Modified carbon black applied to coloring spinning resin and preparation method thereof
CN112456467A
Epoxy base paint composition for concrete structure and surface coating method of concrete structure facility using thereof
KR102253520B1