Slick water fracturing fluid as well as preparation method and application thereof
By modifying the slippery water fracturing fluid of silica and chemical additives, the problem of oil and gas flow difficulties in the shale formation is solved, the fracturing performance and salt resistance are improved, and the efficiency of shale oil and gas development is enhanced.
Patent Information
- Application Number
- CN202411205058.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing slippery water fracturing fluid is difficult to flow effectively in the shale formation, making it difficult for oil and gas to flow into the fracture system, reducing the fracturing performance.
By preparing a slippery water fracturing liquid containing modified silica and specific chemical additives, the surface modification and intermolecular network structure of nanomaterials can be used to improve liquid viscosity and salt resistance, ensure uniform dispersion of nanoparticles and self-priming into the nanoparticles Shale low pore and low permeability formation.
It improves the viscosity and salt resistance of the slippery water fracturing fluid, promotes oil and gas flow to the crack system, and enhances the development efficiency of shale oil and gas.
Smart Images

Figure CN119081673A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fracturing fluid, and in particular to a slick water fracturing fluid and a preparation method and application thereof. Background Art
[0002] As traditional oil and gas resources are gradually becoming depleted and energy demand is growing, it is particularly important to increase the exploration and development of unconventional oil and gas resources in order to provide a stable energy base and effectively guarantee energy supply. Since unconventional oil and gas reservoirs generally have the characteristics of low permeability and low porosity, the difficulty of their development is greatly increased. In order to improve mining efficiency and achieve the purpose of economic development, it is necessary to transform unconventional oil and gas reservoirs through hydraulic fracturing technology.
[0003] Slippery water fracturing fluid is a new type of fracturing fluid system currently widely used in unconventional oil and gas development, because its low viscosity allows the fracturing fluid to slowly leak out of the hydraulic fractures, forming many small fractures in the shale formation. Chemical additives for slippery water usually include drag reducers, surfactants, clay stabilizers, etc. Although the existing slippery water fracturing fluid has formed an oil and gas diversion channel, due to the low porosity and low permeability of shale, it is difficult for oil and gas far away from the fracturing fracture system to flow into the fracture system.
[0004] Therefore, improving the fracturing performance of slick water fracturing fluid is an urgent problem to be solved. Summary of the invention
[0005] The purpose of the present invention is to provide a slick water fracturing fluid and a preparation method and application thereof, so as to solve the problems existing in the prior art.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a slick water fracturing fluid, comprising the following raw materials in parts by weight:
[0008] 0.5-1.5 parts of drag reducer, 0.1-0.3 parts of clay stabilizer, 0.03-0.5 parts of drainage aid and 97-99 parts of water;
[0009] The method for preparing the drag reducer comprises the following steps:
[0010] Mixing silica, a silane coupling agent and an alcohol solution to perform a first reaction to obtain modified silica;
[0011] The oil-water mixture and the emulsifier are mixed to obtain a mixed solution, modified silica, acrylamide, methacrylic acid, and 2-acrylamide-2-methylpropane sulfonic acid are added to the mixed solution, the pH of the mixture is adjusted to neutral, an initiator is added, and a second reaction is carried out to obtain a drag reducer.
[0012] Preferably, in the above-mentioned slick water fracturing fluid, the clay stabilizer comprises the following raw materials in parts by weight:
[0013] 10-20 parts of polydimethyldiallylammonium chloride, 35-45 parts of choline chloride, 35-55 parts of water;
[0014] The exhaust agent is one or more of fluorocarbon, sodium dodecylbenzene sulfonate, propanol and isopropanol.
[0015] Preferably, in the above-mentioned slick water fracturing fluid, the amount ratio of the silicon dioxide, the silane coupling agent and the alcohol solution is 3-8 g: 2-5 g: 60-100 mL;
[0016] The temperature of the first reaction is 40-70° C., and the time of the first reaction is 4-8 hours.
[0017] Preferably, in the above-mentioned slick water fracturing fluid, the oil-water mixture consists of white oil and water; the mass ratio of the white oil to water is 5-6:3-4;
[0018] The content of the emulsifier in the mixed solution is 5-10 wt %.
[0019] Preferably, in the above-mentioned slick water fracturing fluid, the mass ratio of the modified silica, acrylamide, methacrylic acid, 2-acrylamide-2-methylpropanesulfonic acid and initiator is 0.01-0.5: 1-20: 0.1-10: 5-30: 0.01-0.1;
[0020] The ratio of the oil-water mixture to the modified silicon dioxide is 5-20:0.01-0.5;
[0021] The initiator is one or both of potassium persulfate and ammonium persulfate;
[0022] The temperature of the second reaction is 30-60° C., and the time of the second reaction is 4-6 hours.
[0023] The present invention also provides a method for preparing a slick water fracturing fluid, comprising the following steps:
[0024] The drag reducer, clay stabilizer, drainage aid and water are mixed and reacted to obtain a slick water fracturing fluid.
[0025] Preferably, in the above-mentioned method for preparing a slick water fracturing fluid, the reaction temperature is 40 to 60° C., and the reaction time is 10 to 30 minutes.
[0026] The present invention also provides an application of slick water fracturing fluid in increasing the production of shale oil and gas.
[0027] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0028] The present invention provides a slick water fracturing fluid, which prevents the aggregation of nanoparticles through surface modification of nanomaterials, so that the nanoparticles are evenly dispersed in the liquid, and the nanoparticles maintain good dispersibility and nanometer size, and can enter the low-porosity and low-permeability strata of shale through self-absorption; the modified nano-SiO2 can be firmly adsorbed and grafted on the main chain of the polymer, thereby improving the temperature resistance of the polymer. At the same time, the modified nanoparticles can also bridge between different molecular main chains to form an intermolecular network structure. The formation of this structure can hinder the occurrence of polymer aggregation, promote the growth of molecular chains, and protect the main chain and side chain of the polymer, thereby achieving the improvement of the viscosity of the fracturing fluid system, salt resistance and other properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for describing the embodiments or the prior art are briefly introduced below.
[0030] Figure 1 The present invention is a flow chart for preparing the drag reducing agent. DETAILED DESCRIPTION
[0031] The present invention provides a slick water fracturing fluid, comprising the following raw materials in parts by weight:
[0032] 0.5-1.5 parts of drag reducer, 0.1-0.3 parts of clay stabilizer, 0.03-0.5 parts of drainage aid and 97-99 parts of water.
[0033] In the present invention, the mass fraction of the drag reducing agent is preferably 0.5 to 1.5 parts, more preferably 0.8 to 1.2 parts, and even more preferably 0.9 to 1 part.
[0034] In the present invention, the mass fraction of the clay stabilizer is preferably 0.1 to 0.3 parts, more preferably 0.15 to 0.25 parts, and more preferably 0.2 to 0.22 parts.
[0035] In the present invention, the weight percentage of the drainage aid is preferably 0.03 to 0.5 parts, more preferably 0.05 to 0.4 parts, and even more preferably 0.1 to 0.3 parts.
[0036] In the present invention, the mass fraction of the water is preferably 97 to 99 parts, more preferably 97.5 to 98.5 parts, and even more preferably 97.8 to 98 parts.
[0037] In the present invention, the clay stabilizer comprises the following raw materials in parts by weight:
[0038] 10-20 parts of polydimethyldiallylammonium chloride, 35-45 parts of choline chloride, and 35-55 parts of water.
[0039] In the present invention, the mass fraction of polydimethyldiallylammonium chloride in the clay stabilizer is preferably 10 to 20 parts, more preferably 12 to 18 parts, and more preferably 15 to 16 parts.
[0040] In the present invention, the mass fraction of choline chloride in the clay stabilizer is preferably 35 to 45 parts, more preferably 36 to 43 parts, and more preferably 38 to 42 parts.
[0041] In the present invention, the mass fraction of water in the clay stabilizer is preferably 35 to 55 parts, more preferably 38 to 50 parts, and more preferably 42 to 45 parts.
[0042] In the present invention, the preparation method of the clay stabilizer comprises the following steps:
[0043] Polydimethyldiallylammonium chloride, choline chloride and water are mixed at room temperature to obtain a clay stabilizer.
[0044] In the present invention, the exhaust agent is preferably one or more of fluorocarbon, sodium dodecylbenzene sulfonate, propanol and isopropanol, further preferably one or more of fluorocarbon, sodium dodecylbenzene sulfonate and propanol, more preferably one or two of fluorocarbon and sodium dodecylbenzene sulfonate.
[0045] In the present invention, the method for preparing the drag reducer comprises the following steps:
[0046] Mixing silica, a silane coupling agent and an alcohol solution to perform a first reaction to obtain modified silica;
[0047] The oil-water mixture and the emulsifier are mixed to obtain a mixed solution, modified silica, acrylamide, methacrylic acid, and 2-acrylamide-2-methylpropane sulfonic acid are added to the mixed solution, the pH of the mixture is adjusted to neutral, an initiator is added, and a second reaction is carried out to obtain a drag reducer.
[0048] In the present invention, the silane coupling agent is preferably vinyltriethoxysilane.
[0049] In the present invention, the usage ratio of the silica, silane coupling agent and alcohol solution is preferably 3-8 g: 2-5 g: 60-100 mL, more preferably 3.5-7.5 g: 2.5-4.5 g: 70-90 mL, and more preferably 4-6 g: 3-4 g: 75-85 mL.
[0050] In the present invention, the concentration of the alcohol solution is preferably 90 to 95 wt %, more preferably 91 to 94 wt %, and even more preferably 92 to 93 wt %.
[0051] In the present invention, the alcohol solution is preferably an ethanol aqueous solution.
[0052] In the present invention, the temperature of the first reaction is preferably 40 to 70°C, more preferably 45 to 65°C, and more preferably 50 to 55°C; the time of the first reaction is preferably 4 to 8 hours, more preferably 4.5 to 7.5 hours, and more preferably 5 to 6 hours.
[0053] In the present invention, after the first reaction is completed, the method further comprises: distilling the obtained product under reduced pressure, washing with ethanol, vacuum filtering, and finally drying at 80° C. for 12 hours.
[0054] In the present invention, the oil-water mixture consists of white oil and water; the mass ratio of the white oil to water is preferably 5-6:3-4, more preferably 5.2-5.8:3.2-3.7, and more preferably 5.4-5.5:3.4-3.5.
[0055] In the present invention, the white oil is preferably No. 5 white oil.
[0056] In the present invention, the emulsifier is preferably one or both of Span-80 and Twen-80.
[0057] In the present invention, the content of the emulsifier in the mixed solution is preferably 5 to 10 wt %, more preferably 6 to 9 wt %, and even more preferably 7 to 8 wt %.
[0058] In the present invention, the mass ratio of the modified silica, acrylamide, methacrylic acid, 2-acrylamide-2-methylpropanesulfonic acid and initiator is preferably 0.01-0.5: 1-20: 0.1-10: 5-30: 0.01-0.10, more preferably 0.02-0.4: 5-15: 1-8: 8-25: 0.02-0.08, and more preferably 0.1-0.3: 8-12: 4-7: 10-20: 0.04-0.07.
[0059] The usage ratio of the oil-water mixture to the modified silicon dioxide is preferably 5-20: 0.01-0.5, more preferably 8-15: 0.02-0.4, and more preferably 10-12: 0.15-0.2.
[0060] In the present invention, the initiator is preferably one or both of potassium persulfate and ammonium persulfate.
[0061] In the present invention, the temperature of the second reaction is preferably 30-60°C, more preferably 35-55°C, more preferably 40-50°C; the time of the second reaction is preferably 4-6h, more preferably 4.5-5.5h, more preferably 5h.
[0062] In the present invention, after the second reaction is completed, the method further comprises: washing the obtained product with anhydrous ethanol, and finally vacuum drying at 90° C. for 12 hours.
[0063] The present invention also provides a method for preparing a slick water fracturing fluid, comprising the following steps:
[0064] The drag reducer, clay stabilizer, drainage aid and water are mixed and reacted to obtain a slick water fracturing fluid.
[0065] In the present invention, the reaction temperature is preferably 40-60°C, more preferably 45-58°C, more preferably 50-55°C; the reaction time is preferably 10-30 min, more preferably 15-25 min, more preferably 20-22 min.
[0066] The present invention also provides an application of slick water fracturing fluid in increasing the production of shale oil and gas.
[0067] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0068] Example 1
[0069] Mixing 15 parts of polydimethyldiallylammonium chloride, 35 parts of choline chloride and 40 parts of water at 25° C. to obtain a clay stabilizer;
[0070] Silica, vinyl triethoxysilane and alcohol solution were mixed and reacted at 60°C for 5 hours. After the reaction, the obtained product was distilled under reduced pressure, washed with ethanol, vacuum filtered, and finally dried at 80°C for 12 hours to obtain modified silica;
[0071] No. 5 white oil and deionized water are mixed in a mass ratio of 6:4 to obtain an oil-water mixture;
[0072] The oil-water mixture and the emulsifier Span-80 are mixed to obtain a mixed solution, and modified silica, acrylamide, methacrylic acid, and 2-acrylamide-2-methylpropanesulfonic acid are sequentially added to the mixed solution to obtain a mixture, and the pH of the mixture is adjusted to 7 with 20wt% sodium hydroxide, and then an initiator potassium persulfate is added, and the mixture is reacted at 40°C for 5 hours. After the reaction is completed, the obtained product is washed with anhydrous ethanol, and finally vacuum dried at 90°C for 12 hours to obtain a drag reducer; wherein the content of the emulsifier Span-80 in the mixed solution is 5wt%; the mass ratio of the modified silica, acrylamide, methacrylic acid, 2-acrylamide-2-methylpropanesulfonic acid and the initiator is 0.2:15:8:20:0.08; the mass ratio of the oil-water mixture to the modified silica is 15:0.2;
[0073] 1.3 parts of drag reducer, 0.3 parts of clay stabilizer, 0.4 parts of drainage aid fluorocarbon and 98 parts of water were mixed and reacted at 40°C for 15 minutes to obtain slick water fracturing fluid.
[0074] Example 2
[0075] Mixing 20 parts of polydimethyldiallylammonium chloride, 35 parts of choline chloride and 35 parts of water at 25° C. to obtain a clay stabilizer;
[0076] The silica, silane coupling agent and alcohol solution were mixed and reacted at 50°C for 7 hours. After the reaction, the obtained product was distilled under reduced pressure, washed with ethanol, vacuum filtered, and finally dried at 80°C for 12 hours to obtain modified silica;
[0077] No. 5 white oil and deionized water are mixed in a mass ratio of 6:4 to obtain an oil-water mixture;
[0078] The oil-water mixture and the emulsifier Twen-80 are mixed to obtain a mixed solution, and modified silica, acrylamide, methacrylic acid, and 2-acrylamide-2-methylpropanesulfonic acid are sequentially added to the mixed solution to obtain a mixture, and the pH value of the mixture is adjusted to 7 by using 20wt% sodium hydroxide, and then an initiator potassium persulfate is added, and the mixture is reacted at 50°C for 4 hours. After the reaction is completed, the obtained product is washed with anhydrous ethanol, and finally vacuum dried at 90°C for 12 hours to obtain a drag reducer; wherein the content of the emulsifier Span-80 in the mixed solution is 5wt%; the mass ratio of the modified silica, acrylamide, methacrylic acid, 2-acrylamide-2-methylpropanesulfonic acid and the initiator is 0.5:10:8:15:0.1; the amount ratio of the oil-water mixture and the modified silica is 18:0.5;
[0079] 1.5 parts of drag reducer, 0.3 parts of clay stabilizer, 0.5 parts of drainage aid fluorocarbon and 97.7 parts of water were mixed and reacted at 50° C. for 20 minutes to obtain slick water fracturing fluid.
[0080] Example 3
[0081] Mixing 12 parts of polydimethyldiallylammonium chloride, 42 parts of choline chloride and 50 parts of water at 25° C. to obtain a clay stabilizer;
[0082] The silica, silane coupling agent and alcohol solution were mixed and reacted at 60°C for 7 hours. After the reaction, the obtained product was distilled under reduced pressure, washed with ethanol, vacuum filtered, and finally dried at 80°C for 12 hours to obtain modified silica.
[0083] No. 5 white oil and deionized water are mixed in a mass ratio of 6:4 to obtain an oil-water mixture;
[0084] The oil-water mixture and the emulsifier Span-80 are mixed to obtain a mixed solution, and modified silica, acrylamide, methacrylic acid, and 2-acrylamide-2-methylpropanesulfonic acid are sequentially added to the mixed solution to obtain a mixture, and the pH value of the mixture is adjusted to 7 by using 20wt% sodium hydroxide, and then an initiator potassium persulfate is added, and the mixture is reacted at 50°C for 5 hours. After the reaction is completed, the obtained product is washed with anhydrous ethanol, and finally vacuum dried at 90°C for 12 hours to obtain a drag reducer; wherein the content of the emulsifier Span-80 in the mixed solution is 5wt%; the mass ratio of the modified silica, acrylamide, methacrylic acid, 2-acrylamide-2-methylpropanesulfonic acid and the initiator is 0.5:10:7:25:0.1; the amount ratio of the oil-water mixture and the modified silica is 12:0.5;
[0085] 0.5 parts of drag reducer, 0.3 parts of clay stabilizer, 0.2 parts of drainage aid fluorocarbon and 99 parts of water were mixed and reacted at 40°C for 25 minutes to obtain slick water fracturing fluid.
[0086] Performance Testing
[0087] The drag reduction rate, surface tension, anti-swelling rate, interfacial tension, viscosity reduction efficiency and oil displacement efficiency of the slick water fracturing fluids obtained in Examples 1 to 3 were tested respectively according to the petroleum and natural gas industry standards SY / T5107-2016, SY / T5370-2018 and SY / T5971-2016, and the test results are shown in Table 1.
[0088] Table 1 Performance test results of slick water fracturing fluid in Examples 1 to 3
[0089]
[0090]
[0091] Heat and salt resistance
[0092] Salt resistance test method: 10wNaCl+5kCaCl2·2H2O simulated brine was selected to dilute the slick water fracturing fluid prepared in Examples 1 to 3 to the same concentration (0.15wt%), and the dispersion stability of the dilution was observed at room temperature. The drag reduction rate test result after 7 days was used as the evaluation standard. The test results are shown in Table 2; Temperature resistance test method: 10wNaCl+5kCaCl2·2H2O simulated brine was selected to dilute the slick water fracturing fluid prepared in Examples 1 to 3 to the same concentration (0.15%), and the dilution was placed in a 90°C oven. The drag reduction rate test result after 3 days was used as the evaluation standard. The test results are shown in Table 3:
[0093] Table 2 Salt tolerance test results of slick water fracturing fluid in Examples 1 to 3
[0094] 0d stability 0d drag reduction rate 7d stability 7d drag reduction rate Example 1 Uniform 75.3% Uniform 71.4% Example 2 Uniform 76.1% Uniform 72.5% Example 3 Uniform 77.4% Uniform 73.1%
[0095] Table 3 Test results of temperature resistance of slick water fracturing fluid in Examples 1 to 3
[0096] temperature 0d drag reduction rate 3d drag reduction rate Example 1 90℃ 75.3% 71.8% Example 2 90℃ 76.1% 72.9% Example 3 90℃ 77.4% 74.1%
[0097] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A slick water fracturing fluid, It is characterized in that The preparation comprises the following raw materials in parts by weight: 0.5-1.5 parts of drag reducer, 0.1-0.3 parts of clay stabilizer, 0.03-0.5 parts of drainage aid and 97-99 parts of water; The method for preparing the drag reducer comprises the following steps: Mixing silica, a silane coupling agent and an alcohol solution to perform a first reaction to obtain modified silica; The oil-water mixture and the emulsifier are mixed to obtain a mixed solution, modified silica, acrylamide, methacrylic acid, and 2-acrylamide-2-methylpropane sulfonic acid are added to the mixed solution to obtain a mixture, the pH of the mixture is adjusted to neutral, an initiator is added, and a second reaction is carried out to obtain a drag reducer.
2. The slick water fracturing fluid according to claim 1, It is characterized in that The clay stabilizer comprises the following raw materials in parts by weight: 10-20 parts of polydimethyldiallylammonium chloride, 35-45 parts of choline chloride, 35-55 parts of water; The exhaust agent is one or more of fluorocarbon, sodium dodecylbenzene sulfonate, propanol and isopropanol.
3. The slick water fracturing fluid according to claim 2, It is characterized in that The usage ratio of the silicon dioxide, the silane coupling agent and the alcohol solution is 3-8 g: 2-5 g: 60-100 mL; The temperature of the first reaction is 40-70° C., and the time of the first reaction is 4-8 hours.
4. The slick water fracturing fluid according to claim 3, It is characterized in that The oil-water mixture is composed of white oil and water; the mass ratio of the white oil to water is 5-6:3-4; The content of the emulsifier in the mixed solution is 5-10 wt %.
5. The slick water fracturing fluid according to claim 4, It is characterized in that The mass ratio of the modified silica, acrylamide, methacrylic acid, 2-acrylamide-2-methylpropanesulfonic acid and initiator is 0.01-0.5: 1-20: 0.1-10: 5-30: 0.01-0.1; The mass ratio of the oil-water mixture to the modified silicon dioxide is 5-20:0.01-0.5; The initiator is one or both of potassium persulfate and ammonium persulfate; The temperature of the second reaction is 30-60° C., and the time of the second reaction is 4-6 hours.
6. The method for preparing the slick water fracturing fluid according to any one of claims 1 to 5, It is characterized in that The following steps are involved: The drag reducer, clay stabilizer, drainage aid and water are mixed and reacted to obtain a slick water fracturing fluid.
7. The method for preparing the slick water fracturing fluid according to claim 6, It is characterized in that The reaction temperature is 40-60° C., and the reaction time is 10-30 min.
8. Use of the slick water fracturing fluid according to any one of claims 1 to 5 in increasing the production of shale oil and gas.