Etching solution for selectively removing TiSiN and preparation method thereof

By using a combination of inorganic acid, oxidant, inhibitor and surfactant in the etching solution, efficient selective etching of TiSiN is achieved, and the problems of low etching rate and insufficient material selectivity in the prior art are solved, ensuring that Effective processing of semiconductor devices.

CN119081700APending Publication Date: 2024-12-06HUBEI SINOPHORUS ELECTRONIC MATERIALS CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411006744.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

When the existing etching liquid removes TiSiN, the etching rate is low and the selectivity for surrounding materials is insufficient, and there are unknown residues, which affects subsequent use.

Method used

Using an etching solution composed of inorganic acids, oxidants, inhibitors and surfactants, a uniform solution is formed by ultrasonic stirring, and contacting the semiconductor device at a specific temperature and stirring rate, using the action of inhibitors and surfactants to achieve selectivity. Etching.

Benefits of technology

The etching rate of TiSiN is improved while maintaining minimum erosion to the underlying semiconductor material, ensuring the uniformity and integrity of the etching and reducing unidentified residues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses an etching solution for selectively removing TiSiN and a preparation method of the etching solution. The etching liquid mainly comprises inorganic acid, an oxidizing agent, an inhibitor, a surfactant and water. The etching solution not only can effectively remove the TiSiN layer in the semiconductor device, but also can keep the minimum erosion to the bottom semiconductor material structure, thereby improving the selection ratio and production efficiency in the semiconductor manufacturing process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electronic chemicals, and in particular relates to an etching solution for selectively removing TiSiN and a preparation method thereof. Background Art

[0002] With the continuous reduction of technology nodes in the semiconductor field and the increasing requirements for device performance, the performance requirements for materials have reached an unprecedented level. Although materials such as titanium nitride (TiN) commonly used in traditional semiconductor manufacturing perform well in improving conductivity and corrosion resistance, their limitations gradually emerge when facing smaller feature sizes, higher integration density and more complex device structures, especially in terms of thermal stability, interface matching and wear resistance. As a class of advanced thin film materials, titanium silicon nitride (TiSiN) not only inherits the good conductivity and chemical stability of TiN, but also incorporates the high hardness and wear resistance brought by silicon elements and good compatibility with silicon-based semiconductors, thus showing significant advantages in multiple key manufacturing links. At present, TiSiN has been widely studied as a barrier layer in high-k metal gate stacks. Its excellent electrical insulation and thermal stability help maintain the integrity and electrical performance of the gate structure, which is crucial for improving the switching speed of transistors and reducing power consumption. However, due to its high stability and wear resistance, its subsequent removal process has become a major problem.

[0003] Existing etching solutions for removing TiN are mainly composed of oxidants, acids, additives and water. For example, CN114350365 A discloses an etching solution for titanium nitride containing an oxidant, sulfuric acid, a chelating agent, a corrosion inhibitor and a surfactant. CN 114369462 A discloses an etching solution containing hydrogen peroxide, an inorganic acid, a corrosive agent, an etching inhibitor, a surfactant and deionized water. However, when the above-mentioned etching solution is used to remove TiSiN, the obtained etching rate is usually low, so that its selectivity for surrounding materials cannot be satisfied, and after the etching is completed, there are some unidentified residues in the solution, which affects subsequent use. Therefore, there is an urgent need for an etching composition in the art, the purpose of which is to provide an etching solution capable of selectively removing TiSiN and a preparation method thereof, which can increase the TiSiN etching rate while maintaining high selectivity for surrounding materials. Summary of the invention

[0004] The present invention aims to provide an etching solution and a preparation method thereof, which can selectively remove the TiSiN layer in a semiconductor device while maintaining minimal erosion of underlying semiconductor materials such as silicon (Si), silicon dioxide (SiO2) and silicon nitride (Si3N4) structures.

[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is: from about 5 wt % to about 20 wt % of an inorganic acid; from about 20 wt % to about 60 wt % of an oxidizing agent; from about 0.01 wt % to about 1 wt % of an inhibitor; from about 0.01 wt % to about 1 wt % of a surfactant; The balance is high purity water.

[0006] In the above scheme, the inorganic acid is selected from one or more of phosphoric acid, sulfuric acid, hydrochloric acid, fluorosilicic acid and fluoroboric acid, among which the most preferred inorganic acid is phosphoric acid.

[0007] In the above scheme, the oxidant is selected from one or more oxides of peroxides, persulfates, perborates, permanganates, periodates, potassium dichromate, nitric acid, etc. and mixtures thereof, wherein the most preferred oxidant is hydrogen peroxide.

[0008] In the above scheme, the inhibitor can be selected from one or more of vinyl tri(β-methoxyethoxy)silane (VTMOES), allyl tri(trimethylsiloxy)silane (ATMS), styrene ethyl trimethoxysilane (SETMS) and methyl styrene silane (MPS).

[0009] In the above scheme, the mechanism of action of the inhibitor is to release alcohol or other small molecules through a hydrolysis reaction to form highly reactive silanol (Si-OH). This process enables silane to be firmly adsorbed on the surface of silicon-based substances, and the double bond structure makes it more reactive, and can change the surface properties of silicon-based substances more quickly and controllably through a three-dimensional network structure formed by a cross-linking reaction, so that the surface changes from hydrophilic to hydrophobic, thereby reducing direct contact and erosion of the surface by hindering the etching solution from etching it outward through the hydrophobic end with larger steric hindrance.

[0010] In the above scheme, the surfactant is selected from at least one of cationic surfactants such as hexadecyltrimethylammonium bromide (CTAB), polyethyleneimine (PEI), benzyldimethyldodecylammonium chloride, etc.; anionic surfactants such as dodecylbenzenesulfonic acid and its sodium salt, sodium dodecyl sulfate, sodium dodecylbenzenesulfonate (SDBS), etc.; zwitterionic surfactants such as dodecylaminopropionic acid, dodecyldimethylbetaine (BS-12), etc.; nonionic surfactants such as diethylene glycol butyl ether (BDG), polyethylene glycol (PEG), n-octanol, etc.

[0011] In the above scheme, the surfactant further improves the wettability of the surface by reducing the surface tension of the etching solution, thereby improving the uniformity and integrity of the etching.

[0012] Another technical solution of the present invention is to provide an etching method using a TiSiN etching solution, comprising the following steps: S1: adding the above inhibitor and surfactant to the inorganic acid in sequence, and forming a uniform and stable solution by ultrasonic stirring; S2: adding an oxidant to the above solution, adding water to adjust the total amount of the etching solution, and stirring thoroughly to obtain the etching solution.

[0013] S3: contacting a composite semiconductor device including TiSiN, SiO2, Si3N4 and Si with the etching solution and rinsing the semiconductor device after at least partially removing TiSiN.

[0014] The contacting step can be performed in any suitable manner, such as immersion, spraying or flow process. The temperature of the etching solution during the contacting step is preferably about 25°C to about 85°C, more preferably about 65°C to about 85°C. The stirring rate of the etching solution during the contacting step is preferably 100r / min-500r / min, more preferably 300r / min~500r / min. The contact time can be any time from 1 minute to 60 minutes.

[0015] The rinsing step after the contacting step may be performed by any suitable means, such as rinsing the substrate with deionized water by immersion or running water.

[0016] The drying step after the rinsing step can be performed by any suitable means, such as isopropyl alcohol (IPA) vapor drying, heating or blowing with N2.

[0017] Beneficial effects of the present invention The advantages and beneficial effects of the present invention are as follows: in the present invention, the strong oxidizing property of hydrogen peroxide first oxidizes TiSiN, and then the solubility of phosphoric acid combined with the combined action of an inhibitor and a surfactant enables it to be effectively etched, thereby achieving effective removal of the TiSiN layer in the semiconductor device while maintaining minimal erosion of the underlying semiconductor material structure. DETAILED DESCRIPTION

[0018] The technical solutions in the present invention are described clearly and completely below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] 1. Preparation method: According to the components and contents of the embodiments and comparative examples in Table 1, the corresponding raw materials are weighed by percentage calculation, the inhibitor and surfactant are first added to the inorganic acid in sequence, and a uniform and stable solution is formed by ultrasonic stirring, and then the oxidant is added to the above solution and water is added to adjust the total amount of the etching solution, and a uniformly mixed etching solution is obtained after sufficient stirring, wherein the content unit is w%.

[0020] 2. Etching conditions: 25~85℃, stirring and immersing at 300r / min.

[0021] 3. Etching rate detection method: The test pieces containing TiSiN, SiO2, Si3N4 and Si were cut into 1cm*1cm squares during the test, and the film thickness of TiSiN, SiO2, Si3N4 and Si before and after etching was detected using an ellipsometer. The difference between the initial thickness and the thickness after etching divided by the etching time is the etching rate. The results of the embodiments and comparative examples are summarized in Table 2.

[0022] Table 1 shows the components and contents of the etching solutions of Examples 1 to 11 and Comparative Examples 1 to 6

[0023] Table 2 Etching rates and selectivity of etching solutions of Examples 1 to 11 and Comparative Examples 1 to 6

[0024] The above is a detailed description of an etching solution for selectively removing TiSiN and a preparation method thereof of the present invention. The above is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. On the basis of the present invention, some modifications or improvements can be made thereto, which is obvious to those skilled in the art. Therefore, these modifications or improvements made without departing from the spirit of the present invention all belong to the scope of protection claimed by the present invention.

Claims

1. An etching solution for removing TiSiN, characterized in that: The etching solution comprises: from about 5 wt % to about 20 wt % of an inorganic acid; from about 20 wt % to about 60 wt % of an oxidizing agent; from about 0.01 wt % to about 1 wt % of an inhibitor; from about 0.01 wt % to about 1 wt % of a surfactant; The balance is high purity water.

2. The etching solution for removing TiSiN according to claim 1, characterized in that: The inorganic acid is selected from one or a mixture of two or more of phosphoric acid, sulfuric acid, hydrochloric acid, fluorosilicic acid and fluoroboric acid.

3. The etching solution for removing TiSiN according to claim 1, characterized in that: The oxidant is selected from one or a mixture of two or more of peroxide, persulfate, perborate, permanganate, periodate, potassium dichromate and nitric acid.

4. The etching solution for removing TiSiN according to claim 1, characterized in that: The inhibitor is selected from one or a mixture of two or more of vinyl tri(β-methoxyethoxy)silane (VTMOES), allyl tri(trimethylsiloxy)silane (ATMS), styrene ethyl trimethoxysilane (SETMS) and methyl styrene silane (MPS).

5. The etching solution for removing TiSiN according to claim 1, characterized in that: The surfactant is selected from one or a mixture of two or more of cetyltrimethylammonium bromide CTAB, polyethyleneimine PEI, benzyldimethyldodecylammonium chloride, dodecylbenzenesulfonic acid and its sodium salt, sodium dodecyl sulfate, sodium dodecylbenzenesulfonate SDBS, dodecylaminopropionic acid, dodecyldimethylbetaine BS-12, diethylene glycol butyl ether BDG, polyethylene glycol PEG, and n-octanol.

6. An etching method using the etching solution according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1: adding the above inhibitor and surfactant to the inorganic acid in sequence, and forming a uniform and stable solution by ultrasonic stirring; S2: adding an oxidant to the above solution, adding water to adjust the total amount of the etching solution, and stirring thoroughly to obtain the etching solution. S3: contacting the composite semiconductor device comprising TiSiN, SiO2, Si3N4 and Si with the etching solution and rinsing the semiconductor device after at least partially removing the TiSiN.

7. The method according to claim 6, characterized in that The method further includes the step of drying the semiconductor device.

8. The method according to claim 6, characterized in that The contacting step is performed at a temperature of about 25° C. to about 85° C. and a stirring rate of 100 r / min to 500 r / min.

Citation Information

Patent Citations

  • Etching solution for stably etching titanium nitride

    CN114350365A

  • Etching solution for selectively etching titanium nitride and tungsten nitride

    CN114369462A

  • Etching composition and method for fabricating semiconductor device by using the same

    CN108122752A

  • Etching composition and method for fabricating semiconductor device by using the same