Preparation method of novel solid lubricant (NbxTa1-x) 2CSe2

By mixing and heat-treating Nb, Ta, C, Se and polytetrafluoroethylene powders by ball milling, a solid lubricant with a layered structure was prepared, which solved the poor performance of traditional lubricants under harsh conditions. The problem of this method achieves high chemical stability and low friction coefficient effects, and is suitable for a variety of lubrication fields.

CN119081751AActive Publication Date: 2024-12-06INST OF METAL RESEARCH - CHINESE ACAD OF SCI

Patent Information

Application Number
CN202410430066.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-10
Publication Date
2024-12-06
Estimated Expiration
2044-04-10

AI Technical Summary

Technical Problem

Traditional solid lubricants have poor performance under harsh operating conditions such as high temperature, low temperature, vacuum, etc., which is difficult to meet the needs of industrial production. The existing high-performance material preparation methods are complex and are not conducive to industrial production.

Method used

Nb, Ta, C, Se and polytetrafluoroethylene powders were mixed by ball milling, coated with salt shells, and heat treated in a tube-type atmosphere furnace to prepare (NbxTa1-x)2CSe2 solid lubricant with a layered structure, using Van der Waal Force and covalent bonding achieve chemical stability and low friction coefficient of the material.

Benefits of technology

The prepared (NbxTa1-x)2CSe2 solid lubricant has high chemical stability and low friction coefficient. It is suitable for harsh working conditions such as vacuum, low temperature, high temperature, etc., and is simple in process and easy to produce on a large scale.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081751A_ABST
    Figure CN119081751A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of solid lubricants, in particular to a preparation method of a novel solid lubricant (NbxTa1-x) 2CSe2. The method comprises the following steps: (1) weighing Nb powder, Ta powder, C powder, Se powder and polytetrafluoroethylene powder as reactants, putting the reactants into a ball milling tank, adding absolute ethyl alcohol, carrying out ball milling for 2-8 hours, and uniformly mixing; (2) after drying, pressing the mixture into a reactant wafer, coating the surface of the reactant wafer with a layer of KCl and NaCl mixture salt shell, and sealing the reactant wafer coated with the salt shell into a quartz tube; (3) the quartz tube sealed with the reactant wafer is subjected to heat treatment in a tubular atmosphere furnace, the heat treatment temperature is 1000-1300 DEG C, and the heat preservation time is 2-10 h; and naturally cooling to room temperature, and washing to remove salt to obtain the (NbxTa1-x) 2CSe2 solid lubricant. The (NbxTa1-x) 2CSe2 solid lubricating material with high chemical stability and excellent lubricating effect can be prepared through a simple process, and is suitable for harsh working conditions such as vacuum, low temperature, high temperature and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid lubricants, and in particular to a new type of solid lubricant (Nb x Ta 1-x )2CSe2 preparation method. Background Art

[0002] Friction and wear under special working conditions such as high and low temperatures and high vacuum will not only cause huge energy waste in industrial production, but also lead to the failure of mechanical equipment. However, lubricating materials are the most effective means to reduce friction, reduce or avoid wear, and extend the life of mechanical equipment. Lubricating materials are generally divided into liquid lubricants and solid lubricants. Among them, solid lubricants can meet the lubrication requirements under many harsh working conditions such as vacuum, high and low temperatures.

[0003] At present, traditional solid lubricating materials mainly include graphite, molybdenum disulfide, polytetrafluoroethylene, etc. Graphite has extremely poor lubrication performance and wear life in a vacuum environment (Ouyang JH, Li YF, Zhang YZ, et al. High-temperature solid lubricants and self-lubricating composites: A critical review [J]. Lubricants, 2022, 10 (8): 177); while molybdenum disulfide is easily oxidized and decomposed into complex oxides and acidic substances in high temperature and humid environments, resulting in decreased lubrication performance (Vazirisereshk MR, Martini A, Strubbe DA, et al. Solid lubrication with MoS2: a review [J]. Lubricants, 2019, 7 (7): 57); polytetrafluoroethylene is prone to cold flow under high load conditions and is not resistant to radiation (Kumar R, Banga HK, Singh H, et al. An outline on modern day applications of solid lubricants[J].MaterialsToday:Proceedings,2020,28:1962-1967.), therefore, traditional solid lubricants are difficult to meet the requirements of use under extreme working conditions, and it is particularly urgent to develop new solid lubricants for use under harsh conditions.

[0004] Literature (Li Changsheng et al., Research on Friction and Wear Properties of Nano NbSe2-Cu Composite Materials [J]. Mining Engineering, 2008, 28: 79-82) prepared NbSe2 nanomaterials with good friction properties, but the preparation method has high requirements on equipment and low output, which limits its industrial production. Patent (A method for preparing fluorinated graphite solid lubricant) prepares fluorinated graphite with excellent lubrication properties by treating a mixture of graphite and a fluorine source in fluorine gas. Expandable graphite, octafluoropentanol, and fluorine surfactant are used as raw materials and dissolved in a mixed solvent of deionized water and ethylene glycol, ultrasonically promoted emulsification, transferred to a high-pressure reactor for heat treatment, and finally subjected to high-temperature heat treatment in fluorine gas to obtain fluorinated graphite with excellent friction properties. This method uses relatively dangerous fluorine gas, has a long heat treatment time, and has low production efficiency, which is not conducive to large-scale industrial production.

[0005] Layered (Nb x Ta 1-x )2CSe2 is a metallic material formed by atomic covalent bonds of Se-Nb / Ta-C, and its structure is similar to graphite. x Ta 1-x )2CSe2 layers are bound by van der Waals forces and can slip, which theoretically makes (Nb x Ta 1-x )2CSe2 has a lower friction coefficient, and (Nb x Ta 1-x )2CSe2 has excellent thermal stability and other advantages, making (Nb x Ta 1-x )2CSe2 has potential applications in the field of solid lubricants. Summary of the invention

[0006] In order to overcome the shortcomings of the prior art, the present invention provides a new type of solid lubricant (Nb x Ta 1-x )2CSe2 preparation method, through a simple process can be prepared into a solid lubricating material with high chemical stability and excellent lubrication effect, which has potential application prospects under harsh working conditions such as high temperature and low temperature.

[0007] The technical solution of the present invention is:

[0008] A new type of solid lubricant (Nb x Ta 1-x )2CSe2 preparation method, comprising the following steps:

[0009] (1) Weigh Nb powder, Ta powder, C powder, Se powder and polytetrafluoroethylene powder as reactants and place them in a ball mill. The molar ratio of Nb powder, Ta powder, C powder, Se powder and polytetrafluoroethylene powder is (0-2.2):(0-2.2):(0.85-1.2):(1.85-2.5):(0-0.01). Add anhydrous ethanol and ball mill for 2-8 hours to mix well.

[0010] (2) After drying, the mixture is pressed into a reactant disc, and a layer of a mixture of KCl and NaCl salt shell is coated on the surface of the reactant disc, and the reactant disc coated with the salt shell is sealed in a quartz tube;

[0011] (3) The quartz tube sealed with the reactant disc is heat treated in a tubular atmosphere furnace at a temperature of 1000 to 1300°C for a holding time of 2 to 10 hours; after naturally cooling to room temperature, the salt is removed by washing to obtain (Nb x Ta 1-x )2CSe2 solid lubricant.

[0012] The solid lubricant (Nb x Ta 1-x )2CSe2 preparation method, in step (1), the molar ratio of Nb powder and Ta powder to anhydrous ethanol is 1: (0.05~0.1).

[0013] The solid lubricant (Nb x Ta 1-x )2CSe2 preparation method, in step (1), the particle sizes of Nb powder, Ta powder, C powder, Se powder and polytetrafluoroethylene powder are 5-40μm, 5-40μm, 10-60nm, 20-200μm and 100-250nm respectively.

[0014] The solid lubricant (Nb x Ta 1-x )2CSe2 preparation method, in step (2), the diameter of the pressed reactant disc is 8 to 16 mm, and the thickness of the reactant disc is 1 to 10 mm.

[0015] The solid lubricant (Nb x Ta 1-x )2CSe2 preparation method, in step (2), the mass ratio of KCl, NaCl and reactant disc is (0.5~1.5):(0.5~1.5):1.

[0016] The solid lubricant (Nb x Ta 1-x )2CSe2 preparation method, in step (3), the heat treatment adopts a protective atmosphere of a mixture of argon and hydrogen, and the volume ratio of argon and hydrogen is (95~100):(0~5).

[0017] The solid lubricant (Nb x Ta 1-x )2CSe2 preparation method, in step (3), the prepared (Nb x Ta 1-x )The grain size of 2CSe2 solid lubricant is 100~500nm and the thickness is 5~50nm.

[0018] The design idea of ​​the present invention is:

[0019] The synthesized (Nb x Ta 1-x )2CSe2 has a typical two-dimensional layered structure. x Ta 1-x )2CSe2 layers are bound together by weak van der Waals forces, which allow the layers to slide and have a low friction coefficient; while (Nb x Ta 1-x )2CSe2 sheets are made of atomic covalent bonds Se-Nb / Ta-C, which have excellent chemical stability and high and low temperature resistance. x Ta 1-x )2CSe2 as a solid lubricant has broad application prospects under harsh working conditions such as vacuum, low temperature and high temperature.

[0020] The advantages and beneficial effects of the present invention are:

[0021] 1. The solid lubricant (Nb) prepared by the present invention x Ta 1-x )2CSe2 has the advantages of weak interlayer bonding and stable intralayer bonding. The layers are bonded by van der Waals forces, which allows the layers to slip, and the layers are bonded by covalent bonds, which ensures the high chemical stability of the layers. In addition, the synthesis method is simple, easy to operate, and conducive to large-scale production.

[0022] 2. The solid lubricant (Nb x Ta 1-x )2CSe2 has high chemical stability and is resistant to high and low temperatures. It has broad application prospects under harsh working conditions such as vacuum, low temperature and high temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 2 is the XRD spectrum of the solid lubricant Nb2CSe2 prepared in Example 1. In the figure, the abscissa 2θ represents the diffraction angle (°), and the ordinate Intensity represents the diffraction peak intensity (au).

[0024] Figure 2This is the energy spectrum of the solid lubricant Nb2CSe2 in Example 1; wherein a is the high-angle annular dark field image of Nb2CSe2, b is the surface scan of the Nb element, c is the surface scan of the C element, and d is the surface scan of the Se element.

[0025] Figure 3 This is a scanning electron micrograph of the solid lubricant Nb2CSe2 in Example 1.

[0026] Figure 4 (a) and (b) the transmission electron micrograph of the solid lubricant Nb2CSe2 in Example 1.

[0027] Figure 5 This is a high-angle annular dark field image of the solid lubricant Nb2CSe2 at the atomic scale in Example 1.

[0028] Figure 6 The interlayer peeling energy of the conventional solid lubricant (graphite, MoS2) and Nb2CSe2 is compared in this invention, where the vertical axis Binding energy represents the binding energy (J / m 2 ).

[0029] Figure 7 This is the friction coefficient test curve of the solid lubricant Nb2CSe2 in Example 1.

[0030] Figure 8 2 is the XRD spectrum of the solid lubricant Ta2CSe2 prepared in Example 2; in the figure, the abscissa 2θ represents the diffraction angle (°), and the ordinate Intensity represents the diffraction peak intensity (au).

[0031] Fig. 9 This is the energy spectrum of the solid lubricant Ta2CSe2 in Example 1; wherein a is the high-angle annular dark field image of Ta2CSe2, b is the surface scan of the Ta element, c is the surface scan of the C element, and d is the surface scan of the Se element.

[0032] Fig.10 The solid lubricant (Ta 0.5 Nb 0.5 )XRD spectrum of 2CSe2; in the figure, the horizontal axis 2θ represents the diffraction angle (°), and the vertical axis Intensity represents the diffraction peak intensity (au).

[0033] Fig.11 is the solid lubricant (Ta 0.5 Nb 0.5 )Scanning electron micrograph of 2CSe2. DETAILED DESCRIPTION

[0034] In the specific implementation process, the present invention proposes a new type of solid lubricant (Nb x Ta 1-x The preparation method of )2CSe2 comprises the following steps: (1) mixing niobium powder (Nb), tantalum powder (Ta), carbon powder (C), selenium powder (Se) and polytetrafluoroethylene powder (PTFE) and other reactants uniformly by ball milling, and then pressing the reactant disc coated with salt shell (sodium chloride and potassium chloride); (2) heat-treating the reactant disc coated with salt shell in a tubular atmosphere furnace, cooling naturally to room temperature, removing sodium chloride and potassium chloride, and obtaining a novel solid lubricant powder (Nb x Ta 1-x )2CSe2, preferably x = 0 to 1. The solid lubricant prepared by this method (Nb x Ta 1-x )2CSe2 has high chemical stability, and its preparation process is simple and fast, making it easy to commercialize.

[0035] In order to make the contents of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. However, the following embodiments are merely simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0036] The feasibility of the present invention is further verified by examples below.

[0037] Example 1

[0038] In this embodiment, the specific steps of the preparation method of a new type of solid lubricant Nb2CSe2 are as follows:

[0039] (1) 9.3 g of Nb powder, 0.6 g of C powder, 7.9 g of Se powder and 0.67 g of polytetrafluoroethylene powder were weighed as reactants, respectively. The particle sizes of Nb powder, C powder, Se powder and polytetrafluoroethylene powder were 40 μm, 20 nm, 200 μm and 200 nm, respectively. The reactants were placed in a ball mill, 10 mL of anhydrous ethanol was added, and the reactants were ball milled for 4 h. After drying, 1 g of the reactants were weighed and pressed into a reactant disc with a diameter of 10 mm and a thickness of 1 mm. Then, a layer of salt shell was coated on the surface of the reactant disc. A mixture of NaCl and KCl was selected as the salt shell. The mass ratio of NaCl to KCl was 1:1, and the mass ratio of the salt shell to the mass of the reactant was 1:1. Finally, the reactant disc coated with the salt shell was sealed in a quartz tube.

[0040] (2) The quartz tube sealed with the reactant disc is placed in a tube furnace for heat treatment at 1250°C for 6 hours under an Ar / H2 (100 Vol.% + 0 Vol.%) protective atmosphere. After naturally cooling to room temperature, the solid lubricant Nb2CSe2 is washed to remove the salt. The prepared Nb2CSe2 solid lubricant has a grain size of 200 nm and a thickness of 20 nm.

[0041] like Figure 1 As shown, the XRD spectra are the experimental data of Nb2CSe2 and the theoretical simulation data, respectively. The comparison confirms that the experimental data of Nb2CSe2 is consistent with the theoretical simulation, indicating that pure phase Nb2CSe2 has been prepared;

[0042] like Figure 2 As shown in a, it can be seen from the high-angle annular dark field image of Nb2CSe2 that Nb2CSe2 is a regular hexagonal shape. Figure 2 As shown in bd, it can be seen from the surface scan of Nb, C, and Se elements of Nb2CSe2 that the above three elements are evenly distributed on the hexagonal flakes of Nb2CSe2, which also confirms that Nb2CSe2 has been synthesized;

[0043] like Figure 3 As shown, the synthesized Nb2CSe2 samples are all two-dimensional flake structures, most of which are hexagonal in shape, and a few are long strips;

[0044] like Figure 4 As shown in a, from the transmission electron micrograph of Nb2CSe2, an obvious layered structure can be observed; Figure 4 As shown in b, obvious diffraction spots can be seen from the selected area electron diffraction, indicating that the synthesized Nb2CSe2 sample has high crystallinity;

[0045] like Figure 5 As shown, it is a high-angle annular dark field image with atomic resolution of Nb2CSe2, which shows the distribution of Nb2CSe2 atoms, arranged in the form of Se-Nb-C-Nb-Se, and the layers are bonded by van der Waals forces, indicating that the bonding within the layers is stable;

[0046] like Figure 6 As shown, the interlayer bonding strength of traditional solid lubricants graphite, MoS2 and Nb2CSe2 was compared, and it was found that the interlayer bonding energy of these materials is comparable, and the interlayer bonding of Nb2CSe2 is slightly stronger, indicating that Nb2CSe2 is also suitable as a solid lubricant.

[0047] like Figure 7 As shown, we tested the friction coefficient of Nb2CSe2 and found that the friction coefficient of this material is only 0.175, which is significantly lower than that of traditional solid lubricant graphite (the friction coefficient of graphite is 0.23).

[0048] Example 2

[0049] In this embodiment, the specific steps of the preparation method of a new type of solid lubricant Ta2CSe2 are as follows:

[0050] The only difference from Example 1 is that 18.1 g Ta powder, 7.9 g Se powder, 0.6 g C powder and polytetrafluoroethylene powder are weighed as reactants, and the particle sizes of Ta powder, C powder, Se powder and polytetrafluoroethylene powder are 40 μm, 20 nm, 200 μm and 200 nm respectively. The method steps are the same except that a pure phase Ta2CSe2 solid lubricant can be obtained, such as Figure 8 The prepared Ta2CSe2 solid lubricant grains are in regular flake shape, with a grain size of about 300nm and a thickness of 25nm. Fig. 9 shown.

[0051] Example 3

[0052] In this embodiment, a new type of solid lubricant (Nb 0.5 Ta 0.5 The specific steps of the preparation method of )2CSe2 are as follows:

[0053] The only difference from Example 1 is that 9.1 g Ta powder, 4.7 g Nb powder, 7.9 g Se powder, 0.6 g C powder and polytetrafluoroethylene powder are weighed as reactants, and the particle sizes of Nb powder, Ta powder, C powder, Se powder and polytetrafluoroethylene powder are 40 μm, 40 μm, 20 μm, 200 μm and 200 nm respectively. After heat treatment and natural cooling to room temperature, the solid lubricant (Nb 0.5 Ta 0.5 )2CSe2. Fig.10 As shown, pure phase (Nb 0.5 Ta 0.5 )2CSe2 solid lubricant, its grain size is about 200nm, thickness is about 10nm, such as Fig.11 shown.

[0054] Example 4

[0055] In this embodiment, the specific steps of the preparation method of a new type of solid lubricant Nb2CSe2 are as follows:

[0056] The only difference from Example 1 is that a mixture of NaCl and KCl is selected as the salt shell, the mass ratio of NaCl to KCl is 2:1, and the mass ratio of the salt shell to the reactant is 1:2; finally, the reactant disc coated with the salt shell is sealed in a quartz tube. In this embodiment, the prepared Nb2CSe2 solid lubricant has a grain size of 300nm and a thickness of 20nm.

[0057] The results of the examples show that the new solid lubricant (Nb x Ta 1-x )2CSe2 is simple, fast and inexpensive to prepare, and (Nb x Ta 1-x )2CSe2 has a typical layered structure. The layers are bonded by van der Waals forces and can slip. The layers are bonded by Se-Nb / Ta-C-Nb / Ta-Se covalent bonds, which makes the layers have high chemical stability. x Ta 1-x )2CSe2 has potential applications as a solid lubricant in harsh working conditions such as vacuum, low temperature, and high temperature. The present invention is applicable to a variety of lubrication fields - lubricant additives, solid lubricant coatings, etc., especially in the field of solid lubrication technology, and has broad application prospects.

[0058] The above description is only a preferred embodiment of the present invention, but the implementation of the present invention is not limited to the above embodiment. Any obvious improvement, replacement, or modification made by a person skilled in the art on the basis of the present invention shall fall within the protection scope of the present invention.

Claims

1. A new type of solid lubricant (Nb x Ta 1-x )2CSe2 preparation method, characterized in that, The steps include: (1) Weigh Nb powder, Ta powder, C powder, Se powder and polytetrafluoroethylene powder as reactants and place them in a ball mill. The molar ratio of Nb powder, Ta powder, C powder, Se powder and polytetrafluoroethylene powder is (0-2.2):(0-2.2):(0.85-1.2):(1.85-2.5):(0-0.01). Add anhydrous ethanol and ball mill for 2-8 hours to mix well. (2) After drying, the mixture is pressed into a reactant disc, and a layer of a mixture of KCl and NaCl salt shell is coated on the surface of the reactant disc, and the reactant disc coated with the salt shell is sealed in a quartz tube; (3) The quartz tube sealed with the reactant disc is heat treated in a tubular atmosphere furnace at a temperature of 1000 to 1300°C for a holding time of 2 to 10 hours; after naturally cooling to room temperature, the salt is removed by washing to obtain (Nb x Ta 1-x )2CSe2 solid lubricant.

2. The solid lubricant (Nb) according to claim 1 x Ta 1-x )2CSe2 preparation method, characterized in that, In step (1), the molar ratio of Nb powder and Ta powder to anhydrous ethanol is 1:(0.05-0.1).

3. The solid lubricant (Nb) according to claim 1 x Ta 1-x )2CSe2 preparation method, characterized in that, In step (1), the particle sizes of Nb powder, Ta powder, C powder, Se powder and polytetrafluoroethylene powder are 5-40 μm, 5-40 μm, 10-60 nm, 20-200 μm and 100-250 nm respectively.

4. The solid lubricant (Nb) according to claim 1 x Ta 1-x )2CSe2 preparation method, characterized in that, In step (2), the diameter of the pressed reactant disc is 8 to 16 mm, and the thickness of the reactant disc is 1 to 10 mm.

5. The solid lubricant (Nb) according to claim 1 x Ta 1-x )2CSe2 preparation method, characterized in that, In step (2), the mass ratio of KCl, NaCl and reactant disc is (0.5-1.5):(0.5-1.5):

1.

6. The solid lubricant (Nb) according to claim 1 x Ta 1-x )2CSe2 preparation method, characterized in that, In step (3), the heat treatment adopts a protective atmosphere of a mixture of argon and hydrogen, and the volume ratio of argon and hydrogen is (95-100):(0-5).

7. The solid lubricant (Nb) according to claim 1 x Ta 1-x )2CSe2 preparation method, characterized in that, In step (3), the prepared (Nb x Ta 1-x )The grain size of 2CSe2 solid lubricant is 100~500nm and the thickness is 5~50nm.

Citation Information

Patent Citations

  • Preparation method of Nb<1-x>Ta<x>Se<2> nanomaterial

    CN103922293A

  • Preparing method for two-dimensional material

    CN106219608A

  • High temperature Anti-wearing Grease CompositionContaining Solid Lubricant

    KR1020020075958A

Cited By

  • Method for directly synthesizing NbxTa (2-x) S2C material by catalytic method

    CN121269711A