Refining method for reducing size of inclusion in medium-carbon bearing steel and application

By using high alkaline slag to remove oxides and later Si-Al slag adsorption and inclusions in the refining process of medium carbon bearing steel, the problem of large particle inclusions in medium carbon bearing steel is solved, and the cleanliness and fatigue of the steel is improved Performance extends service life.

CN119082405APending Publication Date: 2024-12-06BAOSTEEL SPECIAL STEEL SHAOGUAN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411181990.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

Smart Images

  • Figure CN119082405A_ABST
    Figure CN119082405A_ABST
Patent Text Reader

Abstract

The invention discloses a refining method for reducing the size of inclusions in medium-carbon bearing steel and application, and relates to the technical field of iron and steel smelting. Comprising the steps that molten steel tapped from a converter is refined, the refining process further comprises a slag changing period, and the slag changing period comprises the step that Si-Al refining slag is added into the molten steel. The slag changing period is added in the refining process, before the slag changing period, slag is high in alkalinity and deoxidation capacity, free oxygen in molten steel can be rapidly removed, the cleanliness of the molten steel is improved, and the content of inclusions is reduced; after slag change, the alkalinity of the slag is reduced, the viscosity of the slag is improved, the adsorption capacity to inclusions is improved, large-particle inclusions are completely adsorbed by the slag, most small-particle inclusions are also adsorbed by the slag, the content of the inclusions in molten steel is greatly reduced, the quality and fatigue performance of steel are improved, and the service life of the steel is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of steel smelting, and in particular to a refining method for reducing the size of inclusions in medium-carbon bearing steel and its application. Background Art

[0002] The main function of wheel hub bearings is to bear weight and provide precise guidance for vehicle rotation. Therefore, they need to withstand very large radial loads (vehicle weight) and axial loads (lateral force or lateral impact force borne by the tire when turning) during operation, and are the core of automotive parts. The material used to prepare wheel hub bearings is mainly medium carbon bearing steel. Due to the needs of its service environment, the requirements for steel quality are relatively high. It must have high and uniform hardness and wear resistance, high contact fatigue life, and high elastic limit. Moreover, with the improvement of manufacturing capacity and the increase in customer demand, the market has put forward higher requirements for the quality of bearing steel, especially its excellent fatigue life and quality stability.

[0003] Due to quality control problems during the production process, medium carbon bearing steel is prone to have large particle inclusions in the finished product, which in turn causes fatigue performance failure of the medium carbon bearing steel and reduces its service life. Therefore, how to reduce large particle inclusions in medium carbon bearing steel is a technical problem that needs to be urgently solved in this field.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a refining method and application for reducing the size of inclusions in medium carbon bearing steel.

[0006] The present invention is achieved in that:

[0007] In a first aspect, the present invention provides a refining method for reducing the size of inclusions in medium carbon bearing steel, comprising refining molten steel tapped from a converter, wherein the refining process further comprises a slag changing period, wherein the slag changing period comprises adding Si-Al refining slag to the molten steel;

[0008] Calculated by mass percentage, before the slag transformation period, the slag contains 55-60wt% CaO, 5-8wt% SiO2 and 25-28wt% Al2O3, and the slag basicity is 8-10; after the slag transformation period, the slag contains 40-45wt% CaO, 10-12wt% SiO2 and 32-38wt% Al2O3, and the slag basicity is 4-5.

[0009] In a second aspect, the present invention provides an application of a refining method as described in any one of the aforementioned embodiments in reducing the size of large-particle oxide inclusions in medium-carbon bearing steel.

[0010] The present invention has the following beneficial effects:

[0011] The present invention provides a refining method and application for reducing the size of inclusions in medium-carbon bearing steel. A slag changing period is added during the refining process. Before the slag changing period, the basicity of the slag is relatively high and the deoxidation ability is strong, so the free oxygen content in molten steel can be quickly removed, the cleanliness of the molten steel is improved, and the content of inclusions is reduced. After the slag changing period, the basicity of the slag decreases, the viscosity of the slag increases, the adsorption capacity for inclusions is improved, large-particle inclusions are completely adsorbed by the slag, and most of the small-particle inclusions are also adsorbed by the slag, thereby greatly reducing the content of inclusions in molten steel, improving the quality and fatigue performance of the steel, and increasing the service life of the steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0013] Figure 1 The present invention provides a curve diagram of the mass fraction changes of O, Ca, Mg and Al in the molten steel of the medium carbon bearing steel. DETAILED DESCRIPTION

[0014] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0015] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0016] In a first aspect, the present invention provides a refining method for reducing the size of inclusions in medium carbon bearing steel, comprising refining molten steel produced from a converter, wherein the refining process also includes a slag changing period, and the slag changing period includes adding Si-Al refining slag to the molten steel.

[0017] Calculated by mass percentage, before the slag transformation period, the slag contains 55-60wt% CaO, 5-8wt% SiO2 and 25-28wt% Al2O3, and the slag basicity is 8-10; after the slag transformation period, the slag contains 40-45wt% CaO, 10-12wt% SiO2 and 32-38wt% Al2O3, and the slag basicity is 4-5.

[0018] Please refer to Figure 1 , Figure 1The relationship between the mass fraction changes of O, Ca, Mg and Al in the molten steel of the medium carbon bearing steel provided by the present invention at 1873K is shown.

[0019] Depend on Figure 1 It can be seen that when the Al content in molten steel increases within the range of 0.0025% to 0.06%, the equilibrium O content in the molten steel first decreases and then tends to equilibrium. Therefore, there are limited ways to reduce the O content in molten steel by adding Al to the steel. However, the presence of oxygen will lead to the formation of oxide inclusions, and the growth of these inclusions will directly affect the fatigue service life of the steel, so other methods are needed to remove oxide inclusions in the steel.

[0020] Furthermore, when the Al content in the molten steel increases within the range of 0.0025% to 0.06%, the equilibrium Ca and Mg contents in the molten steel both continue to increase, and the increasing trend of Ca far exceeds the increasing trend of Mg. Therefore, high Al content is more likely to react with CaO to produce CaO-Al2O3 inclusions, so it is necessary to control the Al content to avoid the generation of the above oxide inclusions.

[0021] Since the increase of Mg is relatively slow and its change does not exceed 2.0ppm, the effect of Mg on inclusions can be ignored.

[0022] The present invention proposes slag changing parameters based on the above-mentioned relationship between the mass fraction changes of O, Ca and Mg and Al, so that in the early and middle stages of molten steel refining, high slag basicity is used for strong deoxidation, so that the free oxygen in the molten steel is converted into oxides as much as possible, thereby improving the cleanliness of the molten steel; then, slag changing treatment is used in the later stage of refining to reduce the slag basicity, so that the viscosity of the slag is higher, and the oxides in the molten steel are easily adsorbed into the slag, and the larger the size of the inclusions, the easier they are to be adsorbed by the slag, thereby ensuring that the molten steel has a higher cleanliness, avoiding the presence of large-particle oxide inclusions in the molten steel, improving the fatigue performance of the steel and ensuring the service life of the steel.

[0023] In order to more clearly demonstrate a refining method for reducing the size of inclusions in medium carbon bearing steel provided by the present invention, the method comprises the following steps:

[0024] In an optional embodiment, the refining process includes an alloying pre-deoxidation period, a tank heating period, a slag-making period, a pure refining period and a slag-changing period in sequence.

[0025] After the pure refining period is over and before the slag transformation period begins, the slag contains 55-60wt% CaO, 5-8wt% SiO2 and 25-28wt% Al2O3, and the slag basicity is 8-10.

[0026] After the slag treatment in the slag changing period, the slag contains 40-45wt% CaO, 10-12wt% SiO2 and 32-38wt% Al2O3, and the slag basicity is 4-5.

[0027] S01, alloying pre-deoxidation period

[0028] In an optional embodiment, the alloying pre-deoxidation period sequentially includes the converter steel tapping process and the argon blowing process at the argon station, and the molten steel is sampled after argon blowing at the argon station.

[0029] Specifically, the molten steel at the end of the converter is tapped first. During the tapping process, a portion of slag and alloy raw materials are first added to the molten steel, and a portion is melted in advance, which is beneficial to the full contact between the alloy raw materials and slag and the molten steel; after the converter tapping is completed, the molten steel is sent to the argon station for argon blowing, which promotes the full contact between the alloy raw materials and slag and the molten steel. After the argon blowing is completed at the argon station, the molten steel is sampled. The molten steel sampled at the argon station is used as the basis for adjusting the composition of each element in the subsequent refining process, so that the content of each component in the molten steel at the end of refining meets the requirements of the steel grade.

[0030] In an optional embodiment, the converter steelmaking process includes adding carbon powder to the ladle for the first time, then tapping the converter, adding aluminum iron and a second carbon powder in a subsequent process, and then adding alloy and slag until the converter steelmaking is completed.

[0031] Among them, the carbon powder added for the first time is placed at the bottom of the ladle. During the process of pouring the molten steel from the converter into the ladle, the molten steel is fully in contact with the carbon powder at the bottom of the ladle. The carbon powder can quickly react with the free oxygen in the molten steel to generate carbon dioxide. Combined with the subsequent addition of slag, it can increase the mixing intensity of the slag, improve the slag-melting rate, reduce the original oxygen content in the molten steel, and reduce the proportion of oxide inclusions.

[0032] After the converter has tapped steel for a period of time, for example, when the tapping amount is 40-50 tons of steel, aluminum iron can be added and carbon powder can be added for the second time. The second addition of carbon powder mainly increases the carbon content in the molten steel. When the tapping amount reaches 65 tons, alloy and slag are added. Since the molten steel is stirred rapidly during the converter tapping process, the stirring strength of the slag can be increased, which is conducive to slagging, thereby shortening the argon blowing time of the argon station.

[0033] Aluminum iron and alloys are used as raw materials to adjust the elemental composition of molten steel, and can adjust the content of Al2O3 in the slag, which is conducive to the subsequent adjustment of the composition ratio and slag basicity in the slag. Among them, the type of alloy can be selected according to the requirements of the steel grade. For example, if the elemental composition of the steel grade contains Cr, alloy materials such as ferrochrome can be added.

[0034] Preferably, the mass of the carbon powder added for the first time is 0.6-0.8 kg / ton of steel, and the mass of the carbon powder added for the second time is 2.8-3.2 kg / ton of steel.

[0035] Preferably, the amount of aluminum iron added is 2.0-2.5 kg / ton steel, and the slag includes 2.8-3.2 kg / ton steel of lime and 5.8-6.2 kg / ton steel of pre-melted refined slag.

[0036] Preferably, the mass percentage of carbon in the molten steel at the end of the converter is greater than 0.10wt%, and the mass percentage of oxygen is 200-300ppm.

[0037] Preferably, the temperature of the molten steel at the converter end point is greater than 1610°C, the steel output is 135-140t, and the converter steel output speed is greater than 2s / ton of steel.

[0038] Preferably, during the converter tapping process, the bottom blowing argon flow rate of the ladle is 800-1000 Nm 3 / min.

[0039] Preferably, the mass fraction of Al in the molten steel sampled at the argon station is greater than or equal to 0.035wt%.

[0040] Preferably, the argon flow rate of the argon station is 1800-2200 Nm 3 / min, the argon blowing time of the argon station is 3 to 7 minutes.

[0041] S02, tank heating period

[0042] In an optional embodiment, the refining process during the temperature-raising period includes sending the molten steel to the LF furnace, sending electricity, and blowing argon gas from the bottom. After sending electricity for 1.5 to 2.5 minutes, carbon powder is added to the slag surface of the slag for the third time.

[0043] The purpose of supplying electricity first and then adding carbon powder is to supply electricity first to heat the slag surface and increase the temperature of the slag surface, and then add carbon powder to the slag surface for the third time. Under the high temperature of discharge, the carbon powder on the slag surface can react with the oxygen in the slag and the oxygen in the air to generate carbon dioxide. The overflow of carbon dioxide can increase the foaming properties of the slag and accelerate the melting rate of the slag.

[0044] Preferably, the total refining time during the temperature-raising period is 10 to 15 minutes. After the refining during the temperature-raising period is completed, the temperature of the molten steel is 1520 to 1525°C, more preferably 1520°C.

[0045] Preferably, the power transmission gear during the tank heating period is 8-11 gears, and the bottom blowing argon gas flow rate is 800-1000Nm 3 / min. To ensure that the temperature of the molten steel can be raised to 1520-1525°C within the above refining time.

[0046] In addition, during the temperature-raising period before entering the tank, high-level power transmission and large argon bottom blowing and stirring are used to quickly increase the slag surface temperature and enhance the mixing effect of slag and steel, which is beneficial to the melting of the slag.

[0047] Preferably, the mass ratio of the carbon powder added for the third time to the molten steel is 0.01-0.02:150.

[0048] S03, slag making period

[0049] In an optional embodiment, the refining process in the slag-making stage includes refining the molten steel by maintaining power supply and bottom blowing of argon, and then adding lime, aluminum particles and silicon carbide to the molten steel.

[0050] The steps before the slag-making period are mainly to add the raw materials required for slag-making and the alloy raw materials required for the molten steel, and fully contact these raw materials with the molten steel to melt. The slag-making period is to add the raw materials required for slag-making to the molten steel to obtain the desired slag shape. For example, in the present invention, the desired slag shape must at least meet the following requirements: CaO: 55-60wt%, SiO2: 5-8wt% and Al2O3: 25-28wt% in the slag, and the slag basicity is 8-10. The present invention ensures that the slag shape of the slag meets the requirements by adding lime, aluminum particles and silicon carbide to the molten steel.

[0051] Preferably, during the slag-making period, the diameter of the slag breach is less than 200 mm to avoid excessive slag breach area causing oxygen in the air to enter the molten steel.

[0052] Preferably, the power transmission gear during the slag-making period is 3-4 gears, and the bottom blowing argon gas flow rate is 400-600Nm 3 / min, and the refining time of slag-making period is 10-15min. By reducing the bottom blowing argon flow rate, controlling the diameter of the slag breaking through the air, and maintaining the power transmission process, it is beneficial to slag melting and slag making.

[0053] Preferably, the mass of lime added during the slag-making period is 2.8-3.5 kg / ton of steel; the mass of aluminum particles is 8-12 kg / 150 tons of steel, preferably 10 kg / 150 tons of steel; the mass of silicon carbide is 38-42 kg / 150 tons of steel, preferably 40 kg / 150 tons of steel. Lime can increase the basicity of slag, thereby improving the deoxidation capacity of molten steel. Aluminum particles and silicon carbide are added simultaneously during the process of adding lime. Aluminum particles and silicon carbide can improve the fluidity of slag and avoid lime and slag agglomeration. At the same time, this step can also avoid the use of fluorite, reduce the risk of Ca increase in molten steel, and thus reduce the generation of CaO-Al2O3 inclusions.

[0054] Preferably, after the slag making period, the temperature of the molten steel is 1550-1555°C.

[0055] In an optional embodiment, since the alloy raw materials have all been added to the molten steel in the early stage to adjust the content of each component in the molten steel, after the slag making period is over, the alloy raw materials in the molten steel have been fully melted and mixed with the molten steel. At this time, a molten steel sample is taken as LF sample 1, and the alloy is further fine-tuned according to the elemental composition of LF sample 1, that is, alloy raw materials whose component content does not meet the steel grade requirements are added to the molten steel, and then refining is continued. After the refining is completed, LF sample 2 is taken.

[0056] The mass fraction of Al in the molten steel in LF sample 1 is 0.025-0.030 wt%, and the mass fraction of Al in the molten steel in LF sample 2 is 0.020-0.025 wt%. The composition and basicity of the slag in the refining process can be adjusted by controlling the Al content in the molten steel.

[0057] Preferably, after taking LF sample 1, the power transmission gear is 3-4 gears, and the bottom blowing argon gas flow rate is 800-1000Nm 3 / min, and the refining time is 5 to 10 minutes to melt the raw materials of the alloy added subsequently.

[0058] S04, Pure Refining Stage

[0059] In an optional embodiment, the temperature of the molten steel at the beginning of the pure refining period is 1555-1565°C, the power transmission gear in the pure refining period is 8-11 gears, and the bottom blowing argon gas flow rate is 300-400Nm 3 / min, and the refining time of the pure refining period is 20 to 30 minutes. The high power transmission gear and low bottom blowing flow rate are adopted to fully refine the molten steel in the pure refining period, and at the same time, the refining time of the pure refining period is extended, which is conducive to the collision and growth of oxide inclusions.

[0060] Preferably, the pure refining period also includes adding silicon carbide to the furnace in batches, and the total mass ratio of silicon carbide added in the pure refining period to the mass ratio of molten steel is 0.04-0.05: 150. The purpose of adding silicon carbide in batches is to remove the oxygen content in the slag, and at the same time, carbon dioxide is generated in this process to improve the foamability of the slag.

[0061] S05, slag transformation period

[0062] In the early stage, the oxygen in the molten steel has been transferred to the slag, or converted into large-particle oxide inclusions. The purpose of the slag transformation period is to lock these oxide inclusions in the slag to prevent them from entering the molten steel and ensure the quality of the final steel product.

[0063] Among them, the slag change period includes adding Si-Al refining slag to the molten steel, and Si-Al refining slag includes SiO2 and Al2O3. After adding Si-Al refining slag, the content of corresponding SiO2 and Al2O3 components in the slag increases, the content of CaO decreases, the basicity of the slag decreases, and the viscosity of the slag increases, which is conducive to the adsorption of inclusions.

[0064] In an optional embodiment, the mass ratio of SiO2 to Al2O3 is 1:2.8-3.2; preferably, the mass ratio of SiO2 to Al2O3 is 1:3.

[0065] Preferably, after adding Si-Al refined slag, the mass ratio of CaO to Al2O3 in the slag is 1:0.8-1.2, preferably 1:0.8.

[0066] Preferably, the power transmission gear during the slag change period is 3-4 gears, and the bottom blowing argon gas flow rate is 600-800Nm 3 / min, the refining time in the slag transformation period is 5 to 10min.

[0067] In a second aspect, the present invention provides an application of a refining method as described in any one of the aforementioned embodiments in reducing the size of large-particle oxide inclusions in medium-carbon bearing steel.

[0068] Example 1

[0069] The present embodiment provides a refining method for reducing the size of inclusions in medium carbon bearing steel, wherein the element composition of the medium carbon bearing steel, in terms of mass percentage, includes: C: 0.53-0.58wt%, Si: 0.15-0.30wt%, Mn: 0.75-0.90wt%, P≤0.025wt%, S≤0.008wt%, Cr: 0.12-0.20wt%, Al≤0.050wt%.

[0070] The specific refining process is as follows:

[0071] S01, alloying pre-deoxidation period

[0072] Add 90kg of carbon powder into a ladle with a capacity of 150t and then add the molten steel from the converter into the ladle. During the converter tapping process, the bottom blowing argon flow rate of the ladle is 800-1000Nm 3 / min.

[0073] After the converter taps 45 tons of steel, 2.0kg / ton of aluminum iron, 3.0kg / ton of carbon powder and alloys required by the steel grade are added again. When the tapping amount is about 65 tons, 400kg of lime and 850kg of pre-melted refined slag are added as slag. After the converter tapping is completed, it is sent to the argon station for argon blowing. The argon flow rate is 1800~2200Nm 3 / min, argon blowing time is 5min, then the molten steel is sampled, and the mass fraction of Al in the obtained steel sample is ≥0.035wt%.

[0074] Among them, the mass percentage of carbon in the molten steel at the end of the converter is greater than 0.10wt%, the free oxygen content is 200-300ppm, the molten steel temperature at the end of the converter is greater than 1610℃, the steel output is 135-140t, and the converter steel output is greater than 2s / ton of steel.

[0075] S02, tank heating period

[0076] The molten steel from the argon station is sent to the LF furnace, and then the power is sent at 11 gears and argon is blown from the bottom. The argon flow rate is 800-1000Nm 3 / min. After 2 minutes of power supply, 10kg of carbon powder is added to the slag surface to improve the foaming property of the slag and the deoxidation capacity of the molten steel.

[0077] The total refining time during the heating period is 15 minutes. After the refining is completed during the heating period, the temperature of the molten steel is 1520-1530℃.

[0078] S03, slag making period

[0079] After the tank heating period is over, adjust the power supply gear to gear 4 and adjust the bottom blowing argon gas flow rate to 400-600Nm 3 / min refining for 10min to make slag. During the slag making period, the diameter of the slag breaking through the air is less than 200mm.

[0080] During the slag making process, 400kg lime, 10kg aluminum particles and 40kg silicon carbide are added to the molten steel. After the slag making period, the temperature of the molten steel is 1550-1560℃, the CaO in the slag is 55-60wt%, SiO2 is 5-8wt% and Al2O3 is 25-28wt%, and the slag basicity is 8-10.

[0081] After the slag making period, take the molten steel sample as LF sample 1, and make alloy fine-tuning according to the element composition of LF sample 1. During the alloy fine-tuning process, adjust the power supply gear to 4 gears and the bottom blowing argon gas flow rate to 800-1000Nm 3 / min, and after refining for 10 minutes, the molten steel sample was taken as LF sample 2.

[0082] The mass fraction of Al in the molten steel in LF sample 1 is 0.025-0.030wt%, and the mass fraction of Al in the molten steel in LF sample 2 is 0.020-0.025wt%.

[0083] S04, Pure Refining Stage

[0084] The temperature of the molten steel at the beginning of the pure refining period is 1560-1565℃, the power transmission gear is adjusted to gear 11, and the bottom blowing argon flow rate is 300-400Nm 3 / min, refining for 20 to 30 minutes. During this process, silicon carbide is added into the furnace in batches without adding other raw materials. The total mass of silicon carbide added is 45 kg.

[0085] S05, slag transformation period

[0086] After the pure refining period, the molten steel temperature is 1570℃, the power transmission gear is adjusted to 4 gears, and the bottom blowing argon flow rate is 600~800Nm 3 / min refining for 5 minutes to complete LF refining.

[0087] In this process, Si-Al refined slag is added to the molten steel. After adding the Si-Al refined slag, the slag contains 40-45wt% CaO, 10-12wt% SiO2 and 32-38wt% Al2O3, and the slag basicity is 4-5.

[0088] Comparative Example 1

[0089] This comparative example provides a refining method for medium carbon bearing steel, the element composition of which is the same as that of Example 1, and the specific refining process is as follows:

[0090] S01, alloying pre-deoxidation period

[0091] During the steel-making process of the converter, aluminum iron → alloy → carbon powder → slag are added in the order of alloying.

[0092] The added amounts are 300-350kg of aluminum iron, alloy required for steel grade (total 1300kg), 500kg of carbon powder and slag, wherein the slag includes 800kg of refined slag, 40kg of fluorite and 400kg of lime.

[0093] After the converter is finished tapping, it is sent to the argon station for argon blowing for 10 minutes, with an argon flow rate of 2000Nm 3 / min, and then sample the molten steel. The mass fraction of Al in the molten steel sampled at the argon station is ≥0.020wt%.

[0094] S02, transfer the molten steel from the argon station to the LF furnace

[0095] After entering the tank, power is supplied at 3-4 gears immediately, and argon is blown at the bottom throughout the whole process, with an argon flow rate of 800-1200Nm 3 / min, raise the temperature of molten steel to above 1510℃, add 500-600kg of lime, 50-100kg of fluorite and 150-200kg of SiC at 1520℃ to adjust the slag basicity and fluidity, and remove the residual oxygen in the slag;

[0096] LF sample 1 was taken at 1550°C, and LF sample 2 was taken at 1565°C. The slag composition after LF refining was: CaO: 54~56wt%, SiO2: 8~12wt%, Al2O3: 24~28wt%, R=4~7.

[0097] Test Example 1

[0098] 1) Five batches of medium carbon bearing steel liquid of the same pouring were refined by the methods of Example 1 and Comparative Example 1, and the Al content in the molten steel sampled at the argon station and the slagging effect of the slag in the ladle were detected, as shown in Table 1.

[0099] Table 1 Argon blowing effect of argon station

[0100] Al / wt% in molten steel sampled at the argon station Slag reduction effect Example 1-1 0.031 good Example 1-2 0.036 good Examples 1-3 0.037 good Examples 1-4 0.034 good Examples 1-5 0.040 good Comparative Example 1-1 0.023 Partial clumping Comparative Example 1-2 0.029 good Comparative Examples 1-3 0.031 Partial clumping Comparative Examples 1-4 0.032 good Comparative Examples 1-5 0.025 Partial clumping

[0101] It can be seen from Table 1 that due to the different order of adding the raw materials in the alloying pre-deoxidation period, there are obvious differences in the amount of Al added in the molten steel. The Al content of the embodiment of the present invention is significantly increased, and the slag-removing effect is good and it is not easy to agglomerate. The agglomeration phenomenon of the method in Comparative Example 1 exceeds 50%, and the process control process is more difficult.

[0102] In addition, in the refining process of Comparative Example 1, fluorite is added as one of the raw materials of slag, and the amount of fluorite is large. Fluorite (CaF2) can improve the fluidity of slag and reduce the foaming of slag. When the slag is agglomerated, it can increase the slag-melting rate. However, fluorite cannot increase the basicity of slag, nor can it improve the arc-burying effect of slag. It is very active and can be easily reduced by Al in molten steel to produce CaF2. + Aggravates the formation of large-sized inclusions.

[0103] 2) The above batches of molten steel were further refined according to the corresponding methods of Example 1 and Comparative Example 1 to obtain the refining results shown in Table 2.

[0104] Table 2 Refining effect

[0105]

[0106] As shown in Table 2, the Al and Si contents in the molten steel of LF sample 1 provided by the refining method of the embodiment of the present invention are significantly increased, and the Al content in LF sample 2 is fully controlled within 0.020-0.025%, which can increase the Al2O3 content in the refining slag, reduce the SiO2 content, increase the Al element deoxidation reaction rate in the molten steel, and facilitate the deoxidation of the molten steel. In addition, fluorite is not used in the entire refining process of the embodiment of the present invention, which will not promote the further generation of oxide inclusions, and through more reasonable refining parameter control, the refining time is reduced while ensuring the refining effect, and the refining energy consumption is reduced.

[0107] 3) The composition of the slag when LF sample 1 was sampled and the composition of the slag when LF left the station are shown in Table 3.

[0108] Table 3 Refining slag

[0109]

[0110]

[0111] It can be seen from Table 3 that under the condition that the amount of various raw and auxiliary materials used in the converter steelmaking process is almost the same. The slag basicity of LF sample 1 in the embodiment of the present invention is increased by 4 to 5 compared with the control example, the deoxidation capacity of the molten steel is increased, and the cleanliness of the molten steel is higher. Before the end of the LF stage, the embodiment adopts a slag changing operation. The contents of Al2O3 and SiO2 in the slag leaving the LF station are respectively increased by about 8% and 2% compared with the control example, and the content of CaO is decreased by about 10% compared with the control example. At this time, the fluidity and viscosity of the slag in the embodiment are greatly improved compared with the control example, which is conducive to capturing large-particle oxide inclusions.

[0112] 4) The above 10 batches of molten steel were prepared into medium carbon bearing steel according to the same steps, and the microscopic inclusions of the medium carbon bearing steel were detected, and the results shown in Table 4 were obtained.

[0113] The detection method adopts the extreme value method. Six samples are randomly taken from each batch of medium carbon bearing steel, for a total of 60 samples. Each sample is observed once, and then the observation surface is ground 3mm and observed again. The operation is repeated 12 times in total, with a total of 720 observation surfaces, to observe the inclusions. (The national standard stipulates that the number of inclusions to be tested is 6 per furnace, for a total of 6 results per furnace. The extreme value method is to observe each sample once, then grind and observe again, for a total of 72 results per furnace).

[0114] Table 4 Microscopic inclusions in medium carbon bearing steel

[0115] B coarse>2.0, number Ds>2.5, number Example 1-1 2 0 Example 1-2 1 1 Examples 1-3 1 1 Examples 1-4 1 0 Examples 1-5 0 0 Comparative Example 1-1 3 1 Comparative Example 1-2 6 3 Comparative Examples 1-3 7 4 Comparative Examples 1-4 5 3 Comparative Examples 1-5 4 3

[0116] It can be seen from Table 4 that the medium carbon bearing steel in the embodiment of the present invention has fewer microscopic inclusions and higher cleanliness, so the fatigue performance is better and the service life is increased.

[0117] 5) The above 10 batches of medium carbon bearing steel were subjected to water immersion flaw detection and the test results shown in Table 5 were obtained.

[0118] The method of water immersion flaw detection is: randomly select 5 500mm long sample bars from each furnace of medium carbon bearing steel, totaling 50 bars, and then use SEP 1927-2010-5 level standard for testing. The results are shown in Table 5. Among them, the cleanliness is not up to standard when the sum of the defect volumes of each inclusion in the 500mm long sample bar is greater than 14mm. 3 .

[0119] Table 5 Water immersion flaw detection results of medium carbon bearing steel

[0120]

[0121]

[0122] It can be seen from Table 5 that, under the condition that all raw materials and subsequent tooling equipment are exactly the same, the embodiment of the present invention can further improve the cleanliness of medium carbon bearing steel and control the size of oxide inclusions by adjusting the refining process. The cleanliness of water immersion flaw detection meets the requirements, and the total defect volume meets ≤14mm / dm 3 Compared with the conventional refining method of comparative example 1, the effect is better. In addition, based on the above experimental results, the refining method of the embodiment of the present invention can also reduce the refining cost and improve the refining efficiency, and has great application value.

[0123] The present invention provides a refining method and application for reducing the size of inclusions in medium carbon bearing steel, which has at least the following advantages:

[0124] 1. According to the influence of the change of Al content in molten steel and the balance relationship between Ca, O and Mg, a five-stage smelting method is adopted, including alloying pre-deoxidation period, tank heating period, slag making period, pure refining period and slag changing period, which achieves the effects of carbon deoxidation, aluminum loss preservation, early slag formation, rapid collision and stable removal. The smelting cycle is significantly shortened, the cost is reduced, and the internal quality is improved. This smelting method is conducive to the refined control of the process and is convenient for finding the root cause of the problem.

[0125] 2. Use refined staged Al control technology to inhibit the reduction of CaO in the slag and the increase of Ca in the molten steel + Increase, reduce the risk of oxide inclusions. And use different slag system ratios to interfere with the slag adsorption during the slag change period, increase the control of slag on inclusions, and prevent oxide inclusions that grow up by collision in the later stage of refining from entering the molten steel again. The proportion of large particle levels of B, D, and Ds inclusions can be greatly reduced to produce high-purity medium-carbon bearing steel.

[0126] 3. The B, D, and Ds inclusions in the medium carbon bearing steel obtained by the refining method of the embodiment of the present invention are ≤1.0 level, and the qualified rate is >97%, and the maximum qualified rate can reach 99.6%, which is 3% higher than the original process. The extreme value method is used to compare the inclusions with the original process. The results show that the content of large-particle oxide inclusions in the bearing steel obtained by the method of the embodiment of the present invention is relatively low, which greatly improves the service life of the bearing steel.

[0127] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A refining method for reducing the size of inclusions in medium carbon bearing steel, It is characterized in that The method comprises refining molten steel produced from a converter, wherein the refining process further comprises a slag changing period, wherein the slag changing period comprises adding Si-Al refining slag into the molten steel; Calculated by mass percentage, before the slag transformation period, the slag contains 55-60wt% CaO, 55-60wt% SiO 2 :5~8wt% and Al 2 O 3 :25~28wt%,slag basicity is 8~10;After the slag transformation period, CaO in the slag is 40~45wt%, SiO 2 :10~12wt% and Al 2 O 3 : 32~38wt%, slag basicity is 4~5.

2. The refining method according to claim 1, It is characterized in that The Si-Al refined slag includes SiO 2 and Al 2 O 3 Preferably, SiO 2 and Al 2 O 3 The mass ratio is 1:3; Preferably, after adding the Si-Al refined slag, the CaO and Al in the slag 2 O 3 The mass ratio is 1:0.8-1.2, preferably 1:0.8; Preferably, the power transmission gear in the slag change period is 3-4 gears, and the bottom blowing argon gas flow rate is 600-800Nm 3 / min, and the refining time of the slag transformation period is 5 to 10 minutes.

3. The refining method according to claim 1 or 2, It is characterized in that Before the slag-changing period, the molten steel is refined in sequence through an alloying pre-deoxidation period, a tank-entering temperature-raising period, a slag-making period and a pure refining period.

4. The refining method according to claim 3, It is characterized in that The alloying pre-deoxidation period includes the converter tapping process and the argon blowing process at the argon station in sequence, and the molten steel is sampled after the argon blowing at the argon station; Preferably, the mass fraction of Al in the molten steel sampled at the argon station is greater than or equal to 0.035wt%; Preferably, the argon flow rate of the argon station is 1800-2200 Nm 3 / min, and the argon blowing time of the argon station is 3 to 7 minutes.

5. The refining method according to claim 4, It is characterized in that The converter steel-tapping process includes adding carbon powder to the ladle for the first time, then tapping the converter, adding aluminum and iron in sequence during the converter steel-tapping process, adding carbon powder for the second time, and then adding alloy and slag until the converter steel-tapping is completed; Preferably, the mass of the carbon powder added for the first time is 0.6-0.8 kg / ton of steel, and the mass of the carbon powder added for the second time is 2.8-3.2 kg / ton of steel; Preferably, the amount of aluminum iron added is 2.0-2.5 kg / ton of steel, and the slag material includes 2.8-3.2 kg / ton of steel of lime and 5.8-6.2 kg / ton of steel of pre-melted refined slag; Preferably, the mass percentage of carbon in the molten steel at the end of the converter is greater than 0.10wt%, and the mass percentage of oxygen is 200-300ppm; Preferably, the temperature of the molten steel at the end of the converter is greater than 1610°C, the steel output is 135-140t, and the converter steel output speed is greater than 2s / ton of steel; Preferably, during the converter steel tapping process, the bottom blowing argon flow rate of the ladle is 800-1000 Nm 3 / min.

6. The refining method according to claim 3, It is characterized in that The refining process during the heating period includes sending the molten steel to the LF furnace, sending electricity, and blowing argon gas from the bottom, and adding carbon powder to the slag surface of the slag for the third time after sending electricity for 1.5 to 2.5 minutes; Preferably, the total refining time during the heating period is 10 to 15 minutes, and after the refining during the heating period is completed, the temperature of the molten steel is 1520 to 1525°C; Preferably, the power transmission gear during the tank heating period is 8-11 gears, and the bottom blowing argon gas flow rate is 800-1000Nm 3 / min; Preferably, the mass ratio of the carbon powder added for the third time to the molten steel is 0.01-0.02:

150.

7. The refining method according to claim 3, It is characterized in that The refining process in the slag-making period includes maintaining power supply and bottom blowing argon gas to refine the molten steel, and then adding lime, aluminum particles and silicon carbide into the molten steel; Preferably, during the slag-making period, the diameter of the slag breaking through is less than 200 mm; Preferably, the power transmission gear in the slag-making period is 3-4 gears, and the bottom blowing argon gas flow rate is 400-600Nm 3 / min, the refining time of the slag-making period is 10 to 15min; Preferably, the mass of lime added during the slagging period is 2.8-3.5 kg / ton of steel; the mass of aluminum particles is 8-12 kg / 150 tons of steel; the mass of silicon carbide is 38-42 kg / 150 tons of steel; Preferably, after the slag making period, the temperature of the molten steel is 1550-1555°C.

8. The refining method according to claim 7, It is characterized in that The process comprises sampling the molten steel at the end of the slag-making period as LF sample 1, maintaining power supply and bottom blowing of argon gas and adding alloy raw materials for refining, and taking LF sample 2 after the refining is completed; The mass fraction of Al in the molten steel in LF sample 1 is 0.025-0.030wt%, and the mass fraction of Al in the molten steel in LF sample 2 is 0.020-0.025wt%; Preferably, after taking LF sample 1, the power transmission gear is 3-4 gears, and the bottom blowing argon gas flow rate is 800-1000Nm 3 / min, refining time is 5 to 10min.

9. The refining method according to claim 3, It is characterized in that The temperature of the molten steel at the beginning of the pure refining period is 1555-1565°C, the power transmission gear of the pure refining period is 8-11, and the bottom blowing argon gas flow rate is 300-400Nm 3 / min, the refining time of the pure refining period is 20 to 30min; Preferably, the pure refining period further includes adding silicon carbide into the furnace in batches, and the mass ratio of the total mass of silicon carbide added in the pure refining period to the mass of the molten steel is 0.04-0.05:

150.

10. Use of the refining method according to any one of claims 1 to 9 in reducing the size of large oxide inclusions in medium carbon bearing steel.