Fuel grading pretreatment method, sintering method and application

Through fuel grading pretreatment and lime milk mixing technology, the combustion efficiency and finished product quality of the steel metallurgy sintering process are improved, CO2 and NOx emissions are reduced, and the problems of high energy consumption and large pollutant emissions are solved during the sintering process.

CN119082445APending Publication Date: 2024-12-06HUNAN VALIN XIANGTAN IRON & STEEL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411255657.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing steel metallurgy has high energy consumption and large emissions of gas pollutants during sintering, especially low combustion efficiency under low oxygen content, resulting in an increase in CO and NOx emissions, and the existing denitrification technology is costly and difficult.

Method used

The fuel grading pretreatment method is adopted to classify the solid fuel according to different particle sizes. The first fuel is used for granulation and the second fuel is used for heating. The combustion efficiency and bonding are improved by mixing with lime milk to form a uniform sintered material. The layer temperature field reduces CO2 and NOx emissions.

Benefits of technology

The yield rate and drum strength of sintered ore are improved, and the solid fuel consumption, CO2 and NOx emissions per ton of sintered ore are reduced, achieving low-carbon and low-emission sintering effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005033970600000141
    Figure BDA0005033970600000141
  • Figure BDA0005033970600000142
    Figure BDA0005033970600000142
Patent Text Reader

Abstract

The invention relates to the technical field of ferrous metallurgy sintering, in particular to a fuel grading pretreatment method, a sintering method and application. The fuel grading pretreatment method comprises the following steps: preparing solid fuel into first fuel and second fuel according to particle size distribution; performing first pretreatment on the first fuel to obtain first pretreated fuel; and performing second pretreatment on the second fuel to obtain second pretreated fuel. According to the fuel staged pretreatment method, staged pretreatment is conducted on fuel from the source, the combustion efficiency of solid fuel can be improved, ideal distribution of heat of a sintering material layer is achieved, the purposes of reducing fuel consumption and reducing emission of pollutants such as CO2 and NOx can be achieved, and meanwhile the yield of sintered ore and the strength of a rotary drum can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of iron and steel metallurgy sintering, and in particular to a fuel classification pretreatment method, a sintering method and applications. Background Art

[0002] Sintering is an indispensable process in the existing steel industry, but it has high energy consumption and ranks first in gas pollutant emissions. Energy conservation and emission reduction in the sintering process is a crucial part of achieving clean production in the steel industry.

[0003] The ignition process of sintering uses gas ignition, and the ignition temperature is generally 1000℃~1100℃. The ignition process consumes a lot of oxygen and produces more CO2 and NO. During the ignition process, under the condition of low oxygen content, on the one hand, more CO will be produced; on the other hand, the highest temperature of the combustion zone is low, the mineralization conditions of the upper sintered ore are poor, and the return rate is high; therefore, the combustion efficiency of ignition is reduced under low oxygen content.

[0004] During the sintering process, the main source of flue gas pollutants is the combustion of solid fuels. This is because the temperature difference between the upper and lower layers is large, resulting in incomplete combustion of the upper fuel. The more mature sintering flue gas denitrification technologies currently used are mostly end-of-pipe treatment technologies (SCR, SNCR processes, activated carbon combined desulfurization and denitrification technologies, etc.). These technologies remove NOx after it is generated. However, the sintering flue gas composition is complex and the flue gas volume is large, which makes the catalyst consumption in these technologies large, the processing cost is high, and the difficulty is relatively large. In addition, incomplete fuel combustion not only causes energy waste, but also has an adverse effect on the sintering process. Summary of the invention

[0005] In order to solve the above problems, the present application proposes a fuel graded pretreatment method, a sintering method and an application. The fuel graded pretreatment method is to grade and pretreat the fuel from the source, which can improve the combustion efficiency of solid fuel, realize the ideal heat distribution of the sintering material layer, reduce fuel consumption, and reduce CO2, NO x The purpose of reducing the emission of pollutants such as sintering materials can also be achieved by improving the yield of sintered ore and the strength of the drum.

[0006] This application is implemented through the following technical solutions:

[0007] One of the purposes of the present application is to provide a fuel graded pretreatment method, comprising the steps of:

[0008] Formulating the solid fuel into a first fuel and a second fuel according to a particle size distribution;

[0009] Performing a first pretreatment on the first fuel to obtain a first pretreated fuel;

[0010] performing a second pretreatment on the second fuel to obtain a second pretreated fuel;

[0011] The mass percentage of the particle size distribution of the first fuel includes: 10% to 35% for particle size ≥ 3mm, 50% to 65% for particle size 1mm≤<3mm, and 15% to 25% for particle size <1mm;

[0012] The mass percentages of the particle size distribution of the second fuel include: 30% to 50% for a particle size ≥ 3 mm, 30% to 60% for a particle size 1 mm ≤ < 3 mm, and 10% to 20% for a particle size < 1 mm.

[0013] The fuel grading pretreatment method provided in the present application is characterized in that the first fuel is used for granulation and is placed in the lower sintering material layer during sintering. This particle size distribution is not only conducive to the combustion of the fuel during the sintering process, but also makes the fuel more evenly distributed in the granulated balls as an adhesive powder, fully contacting with the iron ore and flux, thereby producing more calcium ferrite-based bonding phases; the second fuel is placed in the upper material layer during sintering, and is used to supplement heat for the upper sintering material layer. After ignition, more heat of the upper sintering material dissipates into the air. This particle size distribution makes the fuel burn more slowly and the heat release process is more gentle, avoiding the rapid dissipation of heat into the environment after concentrated release.

[0014] In some possible implementations, the first pretreatment includes the step of mixing the first fuel with lime milk.

[0015] In some possible implementations, the mass ratio of the first fuel to the lime milk is 1:(1.5-2.5).

[0016] In some possible implementations, the mass ratio of the first fuel to the lime milk is 1:(2-2.5).

[0017] In some possible implementations, the solid content of the lime milk is 45% to 55%.

[0018] In some possible implementations, the second pretreatment comprises the steps of: mixing the second fuel with lime milk slurry; and the lime milk slurry components include lime milk and iron ore concentrate.

[0019] In some possible implementations, the mass ratio of the second fuel to the lime milk slurry is (2-3):1.

[0020] In some possible implementations, the mass ratio of the second fuel to the lime milk slurry is (2.25-2.75):1.

[0021] In some possible implementations, the preparation of the lime milk slurry includes the steps of: mixing quicklime, iron ore concentrate and water in a mass ratio of 1:(1-2):1 to obtain the lime milk slurry.

[0022] The second object of the present application is to provide a sintering method, comprising the following steps:

[0023] Pretreating the solid fuel according to the pretreating method provided in the present application to obtain the first pretreating fuel and the second pretreating fuel;

[0024] The first pretreated fuel and the raw material to be sintered are formed into a sintering material layer;

[0025] After the second pretreated fuel is distributed on the sintering material layer to form a supplementary heat material layer, ignition and sintering are performed.

[0026] The fuel of the sintering method of the present application is first pretreated by the pretreatment method provided by the present application. The fuel of the sintering method has high combustion efficiency, uniform distribution of the temperature field of the sintering material layer, guaranteed quality of sintered ore, and can achieve an increase of 0.5% to 2% in the sintered ore yield, 1% to 2% in the drum strength, 2kg to 6kg reduction in solid fuel consumption per ton of sintered ore, 16.1% reduction in CO2 emissions, and 10.5% to 20.5% reduction in NO x Emissions reduced by 22.3%.

[0027] In some possible implementations, the mass ratio of the first fuel to the second fuel is: (90-96):(4-10).

[0028] In some possible implementations, the height of the sintering material layer is greater than 900 mm.

[0029] In some possible implementations, the cloth processing comprises the steps of:

[0030] The second pre-treated fuel is laid on a surface of the sintering material layer including a plurality of material grooves to form the supplementary heat material layer.

[0031] In some possible implementations, the depth of the material trench is less than 60 mm.

[0032] In some possible implementations, the mass ratio of the raw material to be sintered to the first pretreated fuel is (27.6-29.5):1.

[0033] In some possible implementations, in the sintering method, the amount of solid fuel added to the raw material is reduced at a ratio of (1.1 to 1.5):1 of the mass ratio of the carbon reduction amount to the second fuel.

[0034] The third purpose of the present application is to provide an application of the sintering method provided in the present application in the field of steel metallurgical sintering. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.

[0036] Obviously, the following descriptions are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in the field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.

[0037] However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the following description is provided for those skilled in the art to fully understand the present application and is not intended to limit the subject matter described in the claims.

[0038] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution, and all technical features and optional technical features of the present application can be combined with each other to form a new technical solution.

[0039] It is generally believed in the art that in the sintering process, fuel with a particle size of 1mm to 3mm has better combustion efficiency. The CO produced during the combustion of solid fuel has the function of reducing NO in the flue gas. x The role of NO, especially under the catalysis of calcium ferrite x The reduction efficiency is increased, and the reaction formula is: Although more CO is produced by fuel combustion during the sintering ignition stage, the produced CO will be quickly drawn into the sintering flue gas and discharged. Therefore, the existence time of CO is short and it cannot be combined with NO x The reaction is fully reacted, and at the same time, it is difficult for calcium ferrite, which has a catalytic effect on the reaction, to be produced on the surface of the sintered material, making NO x The reduction rate is low.

[0040] In order to balance the combustion efficiency of fuel and improve NO x In order to improve the reduction rate and reduce CO emissions at the same time, the embodiments of the present application propose a fuel grading pretreatment method and a sintering method. The fuel grading pretreatment method of the embodiments of the present application shows that when solid fuel is added to the surface of the sintering material layer, fuel of a larger particle size is required to ensure that the high temperature is maintained for a long time in the addition area. If the particle size below 1 mm accounts for a large proportion, the combustion rate is faster, and the faster combustion rate will cause the heat to be released in a concentrated manner and quickly dissipated through the surface of the material layer, thereby affecting the normal sintering. The sintering method of the embodiments of the present application promotes the combustion of solid fuels, increases CO and NO by adopting the methods of fuel screening and grading, pretreatment and addition to the surface of the sintering material. x reaction time, and at the same time enable sintering to be carried out under lower ignition conditions, reduce the amount of gas used and the amount of fuel ingredients in the raw materials, and achieve the purpose of low-carbon and low-emission sintering.

[0041] The following is a detailed description of a fuel grading pretreatment method and a sintering method in an embodiment of the present application.

[0042]

A fuel grading pretreatment method

[0043] One of the purposes of the embodiments of the present application is to provide a fuel graded pretreatment method, comprising the steps of:

[0044] S10. Formulate the solid fuel into a first fuel and a second fuel according to the particle size distribution.

[0045] S20. Perform a first pretreatment on the first fuel to obtain a first pretreated fuel.

[0046] S30. Perform a second pretreatment on the second fuel to obtain a second pretreated fuel.

[0047] In step S10, the mass percentage of the particle size distribution of the first fuel includes: 10% to 35% for particle size ≥ 3 mm, 50% to 65% for particle size 1 mm ≤ < 3 mm, and 15% to 25% for particle size < 1 mm.

[0048] In step S10, the mass percentage of the particle size distribution of the second fuel includes: 30% to 50% for particle size ≥ 3 mm, 30% to 60% for particle size 1 mm ≤ < 3 mm, and 10% to 20% for particle size < 1 mm.

[0049] The fuel grading pretreatment method provided in the embodiment of the present application is characterized in that the first fuel is used for granulation and is the main source of sintering heat. The particle size distribution is not only conducive to the combustion of the fuel during the sintering process, but also makes the fuel more evenly distributed in the granulation balls as an adhesive powder, and fully contacts with the iron ore and flux, thereby producing more calcium ferrite-based bonding phases; the second fuel is used to supplement heat for the upper material layer and reduce the ignition temperature. The particle size distribution makes the fuel burn more slowly and the heat release process is more gentle, thereby avoiding the rapid dissipation of heat into the environment after concentrated release.

[0050] In the embodiment, the mass percentage of the particle size distribution of the first fuel includes: 10% to 35% for particle size ≥ 3mm, 50% to 65% for particle size 1mm≤<3mm, and 15% to 25% for particle size <1mm. In this case, the first fuel used for granulation is the main heat source in the sintering process and is distributed throughout the sintering material layer. When the particle size 1mm≤<3mm accounts for 50% to 65%, the first fuel has better combustibility, and the heat of combustion is not released in a concentrated manner and the loss rate is low, thereby improving the combustion efficiency of the first fuel.

[0051] In the embodiment, the mass percentage of the particle size distribution of the second fuel includes: 30% to 50% for particle size ≥ 3mm, 30% to 60% for particle size 1mm≤<3mm, and 10% to 20% for particle size <1mm. In this case, in the second fuel, particle size ≥ 3mm accounts for 30% to 50%, and particle size 1mm≤<3mm accounts for 30% to 60%. Under the premise of ensuring combustibility, the second fuel can effectively supplement heat to the upper material layer and reduce the ignition temperature.

[0052] In some embodiments, in the above step S10, the solid fuel includes at least one of coke, anthracite, and lignite.

[0053] In some embodiments, in the above step S20, the first pretreatment includes the step of: mixing the first fuel with lime milk. In this case, the mixing of the first fuel and lime milk can increase the adhesion of the first fuel, and at the same time make it easier for the fuel to be coated inside the large particles during the pelletizing process, improve the air permeability of the sintering material layer, and the CO generated in the particles during sintering can have sufficient time to react with NO x reaction; in addition, the lime milk is evenly wrapped on the surface of the first fuel, changing the surface of the first fuel from hydrophobic to hydrophilic, thereby optimizing the granulation performance of the first fuel; further increasing the proportion of large particles after granulation, improving the overall air permeability of the material layer, and thus improving the combustion efficiency of the fuel.

[0054] Permeability: In the sintering of thick material layers, the permeability of the material layer is very important for the normal sintering. With good permeability, enough air can enter the material layer during the sintering process, and there is sufficient O2 to participate in the combustion. Poor permeability will not only significantly reduce the sintering speed, but also make the oxygen potential in the material layer low, the reaction conditions worsen, and it is difficult to generate high-quality calcium ferrite binding phase, which will significantly affect the quality indicators of the sintered ore and seriously hinder the normal sintering.

[0055] In some specific embodiments, the step of mixing the first fuel and lime milk includes: spraying lime milk on the first fuel to obtain a first pretreated fuel. In this case, the lime milk can be evenly coated on the surface of the solid fuel to improve the pelletizing performance of the solid fuel. 2+ Fully contact with iron ore to form calcium ferrite bonding phase, promoting NO x reduction.

[0056] In some embodiments, in the above step S20, the mass ratio of the first fuel to the lime milk is 1:(1.5-2.5). In the exemplary example, it can be a typical but non-limiting mass ratio such as 1:1.5, 1:2.0, 1:2.5, or a range between any two mass ratios. In this case, when the first fuel is used in the pelletizing process, the lime milk is evenly coated on the surface of the first fuel. During pelletizing, the proportion of large particles is increased, and the first fuel is easily coated inside the large particles to improve the air permeability of the sintering material layer; in addition, under this mass ratio range, the fuel can be burned normally, and the particles produced are resistant to NO x The removal effect is good.

[0057] In some embodiments, in the above step S20, the mass ratio of the first fuel to the lime milk is 1:(2-2.5). In the exemplary embodiment, it can be a typical but non-limiting mass ratio such as 1:2, 1:2.5, or a range between any two mass ratios. In this case, the pelletizing performance of the solid fuel is fully optimized, the air permeability of the material layer is improved, the sintered ore index is improved, and NO x Emissions decreased by 16.5% to 22.5%.

[0058] In some embodiments, in the above step S20, the solid content of the lime milk is 45% to 55%. In the exemplary embodiment, it can be 45%, 50%, 55% and other typical but non-limiting solid contents or any range between two solid contents. In this case, the lime milk has a good effect on improving the pelletizing performance of the solid fuel. 2+ It can be evenly distributed on the surface of solid fuel. If the solid content is too low, Ca 2+ If the solid content is too low, the effect of reducing NOx emissions is not obvious. If the solid content is too high, it will hinder the diffusion of O2 to the surface of solid fuel, deteriorate the combustion performance, and have an adverse effect on the sintering process.

[0059] In some embodiments, in the above step S30, the second pretreatment includes the steps of: mixing the second fuel with lime milk slurry; the lime milk slurry components include lime milk and iron concentrate. In this case, the iron concentrate contained in the lime milk slurry can increase the content of calcium ferrite in the material layer, and calcium ferrite can catalyze NO x Reduction; at the same time, the iron concentrate contained in the lime milk slurry also strengthens the mineralization of the upper material layer.

[0060] In some specific embodiments, the step of mixing the second fuel and the lime milk slurry includes: spraying the lime milk slurry into the second fuel to obtain the second pretreated fuel. After the spraying treatment, the contact opportunity between the iron oxide and CaO (calcium hydroxide decomposes into CaO during sintering) can be increased during sintering, and low melting point compounds such as CaO·Fe2O3, 2CaO·Fe2O3, CaO·2Fe2O3, and CaO·FeO·SiO2 are more easily formed between the two, thereby increasing the calcium ferrite content in the upper material layer, which is NO x It provides catalytic effect for the reduction of minerals and strengthens the mineralization effect of the upper material layer.

[0061] The upper material layer refers to the upper 35% area of ​​the sintered material layer.

[0062] In some embodiments, in the above step S30, the mass ratio of the second fuel to the lime milk slurry is (2-3):1. In the exemplary embodiment, it can be a typical but non-limiting mass ratio such as 2:1, 2.5:1, 3:1, or a range between any two mass ratios. In this case, the amount of fuel surface coating is appropriate, so that oxygen and fuel can react and burn normally to generate calcium ferrite, thereby increasing NO x removal efficiency; in addition, this mass ratio can improve the strengthening effect on the upper sintered ore.

[0063] In some specific embodiments, in the above step S30, the mass ratio of the second fuel to the lime milk slurry is (2.25-2.75):1. In the exemplary example, it can be a typical but non-limiting mass ratio such as 2.25:1, 2.5:1, 2.75:1, or a range between any two mass ratios. In this case, the second fuel with a larger particle size and a smaller specific surface area has a more suitable coating effect, and calcium ferrite is generated to promote NO while ensuring the combustion conditions of the fuel. x The second fuel does not participate in the pelletizing process, but is distributed in the sintering material layer as a single particle fuel, mainly to supplement the heat of the upper material layer. Its combustion speed should not be too fast or too slow, and the heat release process should be gentle. Within the mass ratio range of the second fuel and the lime milk slurry, the amount of lime milk coated on the surface of the solid fuel is appropriate, ensuring that a certain amount of O2 diffuses to the fuel surface for reaction, and at the same time sufficient CO is generated to reduce NO under the catalysis of calcium ferrite. x .

[0064] In some embodiments, in the above step S30, the preparation of lime milk slurry includes the steps of: mixing quicklime, iron ore concentrate and water in a mass ratio of 1: (1-2): 1 to obtain lime milk slurry.

[0065] In other embodiments, in the above step S30, the preparation of the lime milk slurry includes the steps of: mixing the lime milk and the iron ore concentrate in a mass ratio of 2:(1-2) to obtain the lime milk slurry.

[0066]

Sintering method

[0067] A second object of the embodiment of the present application is to provide a sintering method, comprising the following steps:

[0068] X10. Pretreat the solid fuel according to the pretreatment method provided in the embodiment of the present application to obtain a first pretreated fuel and a second pretreated fuel.

[0069] X20. Combine the first pretreated fuel and the raw materials to be sintered to form a sintering material layer.

[0070] X30. After the second pretreated fuel is distributed on the sintering material layer to form a supplementary heat material layer, ignition and sintering are performed.

[0071] In the sintering method of the embodiment of the present application, the solid fuel is pretreated by the pretreatment method provided in the embodiment of the present application. The sintering method of the embodiment of the present application has high combustion efficiency of the fuel, uniform distribution of temperature field of the sintering material layer, guaranteed quality of sintered ore, and can achieve an increase of 0.5% to 2% in sintered ore yield, 1% to 2% in drum strength, 2kg to 6kg reduction in solid fuel consumption per ton of sintered ore, 16.1% reduction in CO2 emissions, and 10.5% to 20.5% reduction in NO x Emission reduction of 16.5% to 22.5%.

[0072] In some embodiments, in the above step X10, the mass ratio of the first fuel to the second fuel is: (90-96): (4-10), and in the exemplary example, it can be a typical but non-limiting mass ratio such as 90:10, 95:5, 96:4, or a range between any two mass ratios. In this mass ratio range, the heat of the sintering material layer is sufficient, and the supplementary heat effect on the upper material layer is obvious, which promotes the normal progress of the sintering production.

[0073] In some embodiments, in the above step X20, the height of the sintered material layer is above 900 mm.

[0074] In some embodiments, in the above step X20, the height of the sintering material layer is 920 mm to 1020 mm. In the exemplary embodiment, it can be a typical but non-restrictive height of 920 mm, 990 mm, 1020 mm, or a range between any two heights. In this case, the automatic heat storage effect of the sintering material layer is strong, but the air permeability of the sintering material layer is poor. After the fuel pretreatment, the air permeability of the sintering material layer is improved, and the sintered ore index is improved.

[0075] In some embodiments, in the above step X20, the mass ratio of the raw material to be sintered to the first pretreated fuel is (27.6-29.5):1. In the exemplary embodiment, it can be a typical but non-limiting mass ratio such as 27.6:1, 28:1, 29.5:1, or a range between any two mass ratios.

[0076] In some embodiments, in the above step X20, the raw materials to be sintered include iron ore, dolomite, quicklime, sintering return ore and blast furnace return ore.

[0077] In some embodiments, in the above step X30, the cloth processing includes the steps of:

[0078] The second pre-processed fuel is laid on a surface of a sintering material layer including a plurality of material grooves to form a heat supplementing material layer. In this case, the second pre-processed fuel fills the material grooves and spreads on the surface to form an upper material layer.

[0079] In some embodiments, the depth of the material trench is less than 60 mm. In this case, the solid fuel is more evenly dispersed in the material trench, and the combustion heat release process is relatively smooth and stable.

[0080] In some embodiments, the depth of the trench is less than 50 mm.

[0081] In some embodiments, the depth of the groove is less than 30 mm.

[0082] In some embodiments, the depth of the material groove is 30 mm to 40 mm. In the exemplary embodiment, it can be a typical but non-limiting depth of 30 mm, 35 mm, 40 mm, or a range between any two depths. In this case, within this depth range, the solid fuel has a better distribution state in the material groove. The solid fuel content in the material layer per unit depth will not be too high due to the shallow depth, and the heat will not be released in a concentrated manner. The solid fuel will not be too dispersed due to the deep depth, reducing the heat supplement effect. Within this depth, the solid fuel can be fully ignited during ignition, and the combustion process is relatively smooth, and the heat is relatively sufficient.

[0083] In some embodiments, in the above step X30, in the ignition and sintering step, the ignition temperature is 850° C. to 950° C., and the ignition time is 60s to 120s.

[0084] In some embodiments, in the above step X30, during the ignition and sintering, the ignition temperature is 900° C. to 950° C., and the ignition time is 60 s to 90 s.

[0085] In some embodiments, in the sintering method, the amount of solid fuel added to the raw material is reduced according to a mass ratio of the carbon reduction amount to the second fuel of (1.1-1.5):1.

[0086] The amount of solid fuel added refers to the amount of all solid fuel ingredients including the first fuel and the second fuel. In practical applications, the process of carbon reduction is as follows: after the mass ratio of the first fuel to the second fuel is determined, the amount of the first fuel used can be reduced according to the mass ratio of the carbon reduction to the second fuel. This carbon reduction process is not a mandatory requirement, but under this ratio, it can ensure the sintered ore index while reducing the solid fuel consumption in the sintering process. For example: if ten parts of solid fuel are required, one part of solid fuel is pre-determined and separated as the second fuel during carbon reduction, then only (7.5-7.9) parts of solid fuel need to be added during batching and granulation, and the amount of mixed iron ore, flux, and return ore remains unchanged.

[0087] Raw materials refer to all materials required for granulation and sintering including solid fuel (mixed iron ore, solid fuel, flux, return ore, etc.).

[0088] In some specific embodiments, the mass ratio of the carbon reduction amount to the second fuel is (1.2-1.35):1. In the exemplary embodiment, it can be a typical but non-limiting mass ratio such as 1.2:1, 1.3:1, 1.35:1, or a range between any two mass ratios.

[0089] The following is further described in conjunction with specific embodiments.

[0090] Example 1

[0091] Example 1 proposes a fuel classification pretreatment method, comprising the following steps:

[0092] (1) Coke powder is prepared into a first fuel and a second fuel with a mass ratio of 95:5 according to particle size distribution, wherein the mass percentage of the particle size distribution of the first fuel includes: particle size ≥3 mm is 19%, 1 mm ≤ particle size <3 mm is 61%, and particle size <1 mm is 20%; the mass percentage of the particle size distribution of the second fuel includes: particle size ≥3 mm is 43%, 1 mm ≤ particle size <3 mm is 42%, and particle size <1 mm is 15%.

[0093] (2) lime milk is prepared by using quicklime and water in a mass ratio of 1:1, and the lime milk is sprayed on the first fuel in a mass ratio of 1:2 to the first fuel to obtain a first pretreated fuel.

[0094] (3) lime milk slurry is prepared by using quicklime, iron ore concentrate and water in a mass ratio of 1:1.2:1, and the lime milk slurry is sprayed on the second fuel in a mass ratio of the lime milk slurry to the second fuel of 1:2.5 to obtain a second pretreated fuel.

[0095] This embodiment also provides a sintering method, comprising the following steps:

[0096] 1) The mass fractions of the raw material components are as follows: iron ore 69.29%, light-burned dolomite 3.76%, quicklime 8.06%, sintering return ore 5.08%, blast furnace return ore 10.17%, and coke powder 3.64%.

[0097] 2) The coke powder (with a content of 3.64%) is graded and pretreated according to the fuel graded pretreatment method provided in this embodiment to obtain a first pretreated fuel and a second pretreated fuel, and carbon reduction is performed according to a mass ratio of carbon reduction amount to the second fuel of 1.32:1.

[0098] 3) The first pretreated fuel and other raw materials are mixed and granulated twice to obtain sintering raw meal, and the sintering raw meal is made into a sintering material layer with a material layer height of 1020 mm.

[0099] 4) 15 to 20 grooves with a depth of 30 mm are set on the material surface of the sintering material layer.

[0100] 5) The second pre-treated fuel is distributed on the material surface and in the material groove of the sintering material layer to obtain a supplementary heat material layer.

[0101] 6) After scraping the surface of the heat supplement material layer, set the ignition temperature to 900°C, the ignition time to 90s, and the ignition negative pressure to 5kPa for ignition sintering.

[0102] Example 2

[0103] Example 2 proposes a fuel classification pretreatment method, comprising the following steps:

[0104] (1) Coke powder is prepared into a first fuel and a second fuel with a mass ratio of 95:5 according to particle size distribution, wherein the mass percentage of the particle size distribution of the first fuel includes: particle size ≥3 mm is 16%, 1 mm ≤ particle size <3 mm is 59%, and particle size <1 mm is 25%; the mass percentage of the particle size distribution of the second fuel includes: particle size ≥3 mm is 37%, 1 mm ≤ particle size <3 mm is 49%, and particle size <1 mm is 14%.

[0105] (2) lime milk is prepared by using quicklime and water in a mass ratio of 1:1, and the lime milk is sprayed on the first fuel in a mass ratio of 1:2.5 to the first fuel to obtain a first pretreated fuel.

[0106] (3) lime milk slurry is prepared by using quicklime, iron ore concentrate and water in a mass ratio of 1:1.2:1, and the lime milk slurry is sprayed on the second fuel in a mass ratio of the lime milk slurry to the second fuel of 1:2.75 to obtain a second pretreated fuel.

[0107] This embodiment also provides a sintering method, the steps are basically the same as those in Embodiment 1, except that:

[0108] Step 3) The material layer height is 970 mm.

[0109] Step 4) The depth of the groove is 50 mm.

[0110] In step 6), the ignition temperature is set to 950°C.

[0111] Example 3

[0112] Example 3 proposes a fuel classification pretreatment method, comprising the following steps:

[0113] (1) Coke powder is prepared into a first fuel and a second fuel with a mass ratio of 95:5 according to particle size distribution, wherein the mass percentage of the particle size distribution of the first fuel includes: 26% for particle size ≥3 mm, 51% for particle size 1 mm ≤ <3 mm, and 23% for particle size <1 mm; the mass percentage of the particle size distribution of the second fuel includes: 50% for particle size ≥3 mm, 32% for particle size 1 mm ≤ <3 mm, and 18% for particle size <1 mm.

[0114] (2) lime milk is prepared by using quicklime and water in a mass ratio of 1:1, and the lime milk is sprayed on the first fuel in a mass ratio of 1:2 to the first fuel to obtain a first pretreated fuel.

[0115] (3) lime milk slurry is prepared by using quicklime, iron ore concentrate and water in a mass ratio of 1:1.2:1, and the lime milk slurry is sprayed on the second fuel in a mass ratio of the lime milk slurry to the second fuel of 1:2.25 to obtain a second pretreated fuel.

[0116] This embodiment also provides a sintering method, the steps are basically the same as those in Embodiment 1, except that:

[0117] Step 3) The material layer height is 920 mm.

[0118] Step 4) The depth of the groove is 40 mm.

[0119] In step 6), the ignition time is set to 60s.

[0120] Example 4

[0121] Example 4 proposes a fuel classification pretreatment method, comprising the following steps:

[0122] (1) Coke powder is prepared into a first fuel and a second fuel with a mass ratio of 95:5 according to particle size distribution, wherein the mass percentage of the particle size distribution of the first fuel includes: particle size ≥3 mm is 18%, 1mm≤particle size <3mm is 65%, and particle size <1mm is 17%; the mass percentage of the particle size distribution of the second fuel includes: particle size ≥3 mm is 38%, 1mm≤particle size <3mm is 52%, and particle size <1mm is 10%.

[0123] (2) lime milk is prepared by using quicklime and water in a mass ratio of 1:1, and the lime milk is sprayed on the first fuel in a mass ratio of 1:2 to the first fuel to obtain a first pretreated fuel.

[0124] (3) lime milk slurry is prepared by using quicklime, iron ore concentrate and water in a mass ratio of 1:1.2:1, and the lime milk slurry is sprayed on the second fuel in a mass ratio of the lime milk slurry to the second fuel of 1:2.25 to obtain a second pretreated fuel.

[0125] This embodiment also provides a sintering method, the steps are basically the same as those in Embodiment 1, except that:

[0126] Step 3) The material layer height is 950 mm.

[0127] Step 4) The depth of the groove is 40 mm.

[0128] In step 6), the ignition temperature is set to 1050° C. and the ignition time is set to 60 s.

[0129] Example 5

[0130] Example 5 proposes a fuel classification pretreatment method, comprising the following steps:

[0131] (1) Coke powder is prepared into a first fuel and a second fuel with a mass ratio of 95:5 according to particle size distribution, wherein the mass percentage of the particle size distribution of the first fuel includes: 26% for particle size ≥3 mm, 54% for particle size 1 mm ≤ <3 mm, and 20% for particle size <1 mm; the mass percentage of the particle size distribution of the second fuel includes: 49% for particle size ≥3 mm, 39% for particle size 1 mm ≤ <3 mm, and 12% for particle size <1 mm.

[0132] (2) lime milk is prepared by using quicklime and water in a mass ratio of 1:1, and the lime milk is sprayed on the first fuel in a mass ratio of 1:2 to the first fuel to obtain a first pretreated fuel.

[0133] (3) lime milk slurry is prepared by using quicklime, iron ore concentrate and water in a mass ratio of 1:1.2:1, and the lime milk slurry is sprayed on the second fuel in a mass ratio of the lime milk slurry to the second fuel of 1:2.25 to obtain a second pretreated fuel.

[0134] This embodiment also provides a sintering method, comprising the following steps:

[0135] 1) The mass fractions of the raw material components are as follows: iron ore 69.02%, light-burned dolomite 3.76%, quicklime 8.06%, sintering return ore 5.08%, blast furnace return ore 10.17%, and coke powder 3.90%.

[0136] 2) The coke powder (content of 3.90%) is subjected to graded pretreatment according to the fuel graded pretreatment method provided in this embodiment to obtain a first pretreated fuel and a second pretreated fuel, but the amount of coke powder is not reduced.

[0137] 3) The first pretreated fuel and other raw materials (iron ore, light-burned dolomite, quicklime, sintering return ore and blast furnace return ore) are mixed and granulated twice to obtain sintering raw meal, and the sintering raw meal is made into a sintering material layer with a material layer height of 1000 mm.

[0138] 4) 15 to 20 grooves with a depth of 50 mm are set on the surface of the sintering material layer.

[0139] 5) The second pre-treated fuel is distributed on the material surface and in the material groove of the sintering material layer to obtain a supplementary heat material layer.

[0140] 6) After scraping the surface of the heat supplement material layer, set the ignition temperature to 900°C, the ignition time to 60s, and the ignition negative pressure to 5kPa for ignition sintering.

[0141] Comparative Example 1

[0142] Comparative Example 1 proposes a sintering method, comprising the following steps:

[0143] ① Mix 69.02% iron ore, 3.75% light-burned dolomite, 8.08% quicklime, 5.08% sintering return ore, 10.17% blast furnace return ore and 3.90% coke powder, and mix and granulate them.

[0144] ② After granulation, the material is placed on the sintering trolley, ignited for 60 seconds at a temperature of 1050°C and a negative pressure of 5 kPa, and then sintered at a negative pressure of 14 kPa.

[0145] Comparative Example 2

[0146] Comparative Example 2 proposes a sintering method, comprising the following steps:

[0147] ① The mass fractions of the raw material components are as follows: iron ore 69.29%, light-burned dolomite 3.76%, quicklime 8.06%, sintering return ore 5.08%, blast furnace return ore 10.17%, and coke powder 3.64%.

[0148] ② The coke powder (content of 3.64%) was divided into fuel I and fuel II with a mass ratio of 95:5.

[0149] ③ Fuel I and other raw materials (iron ore, light-burned dolomite, quicklime, sintering return ore and blast furnace return ore) are mixed and granulated twice to obtain sintering raw meal, which is then made into a sintering material layer with a layer height of 1020 mm.

[0150] ④ Set 15 to 20 grooves with a depth of 30 mm on the material surface of the sintering material layer.

[0151] ⑤ Distribute fuel II on the surface and groove of the sintering material layer to obtain a heat supplement layer.

[0152] ⑥ After scraping the surface of the heat supplement material layer, set the ignition temperature to 950℃, the ignition time to 60s, and the ignition negative pressure to 5kPa for ignition sintering.

[0153] In order to verify the progressiveness of the fuel classification pretreatment method and sintering method of the embodiment of the present application, the sintering product quality index (GB 10322.7-2016 Screening determination of iron ore and direct reduced iron particle size distribution, ISO 3271-2015, GB 24205-2009 Iron ore powder sintering test result expression method) of the sintering method proposed in the embodiment and the comparative example, and the detection steps of the pollutant emission reduction index and the maximum temperature of the material layer are as follows. The results are shown in the following Tables 1 to 3 respectively:

[0154] Pollutant emission reduction index detection: A detection hole is opened between each wind box and the large flue, and a portable flue gas analyzer (model: Photon II, with PGD-100 flue gas pretreatment system) is used to detect the flue gas composition. During the detection, after the instrument is preheated and zeroed, the sampling gun is inserted into the detection hole, and wet asbestos rope is wrapped around the hole to reduce air leakage. x After the CO2 reading is stable, continue measuring for 5 minutes, take out the sampling gun and zero the instrument, repeat the above "zeroing-measurement-zeroing" steps 3 times and take the average value as the NO in the flue gas of the bellows. x , CO2 emission test results, test the flue gas of each bellows one by one and record it, and x 、CO2 emissions calculation total NO x , CO2 emissions, and compared with the emissions of comparative example 1, calculate NO x , CO2 emission reduction rate, and keep one decimal place.

[0155] Detection of the maximum temperature of the material layer: Since the temperature of the material layer is difficult to measure during sintering production, the sintering cup method is used to measure the temperature of the material layer under the same raw material conditions and operating system as the embodiments and comparative examples. The method is as follows: holes are opened at 100mm, 300mm, 500mm, and 700mm from the mouth of the sintering cup and 4 K-type thermocouples are set, followed by sintering, and the temperature is recorded when each temperature measuring point reaches the maximum temperature until the sintering cup test is completed. Each group of tests is repeated 3 times and the average value of the maximum temperature of each temperature measuring point is taken as the maximum temperature of the temperature measuring point, and the results are retained as integers.

[0156] Table 1

[0157]

[0158] Table 2

[0159]

[0160] Table 3

[0161] 100mm / ℃ 300mm / ℃ 500mm / ℃ 700mm / ℃ Example 1 1284 1279 1296 1311 Example 2 1303 1281 1295 1323 Example 3 1270 1267 1288 1304 Example 4 1339 1304 1318 1322 Example 5 1278 1263 1313 1330 Comparative Example 1 1136 1210 1271 1305 Comparative Example 2 1251 1248 1264 1293

[0162] From Tables 1 to 3 above, we can at least get:

[0163] (1) As can be seen from Table 1, the fuel is pretreated by the fuel graded pretreatment method of the embodiment of the present application and then sintered, and the sintering yield and drum strength meet the requirements.

[0164] (2) It can be seen from Table 1 that, by using the sintering method of the embodiment of the present application, the reduction in ignition gas per ton of ore decreases as the ignition temperature increases.

[0165] (3) It can be seen from Table 1 that after carbon reduction was carried out in Examples 1 to 4 and Comparative Example 2 at a mass ratio of carbon reduction to the second fuel of 1.32:1, the reduction in solid fuel consumption per ton of sintered ore was greater than 5 kg. However, since no carbon reduction treatment was performed in Example 5 (the amount of coke powder was not reduced), the reduction in solid fuel consumption per ton of sintered ore was lower.

[0166] (4) As can be seen from Table 2, after carbon reduction was performed in Examples 1 to 4 and Comparative Example 2 according to the mass ratio of carbon reduction amount to the second fuel of 1.32:1, the average CO2 emission was reduced.

[0167] (5) As can be seen from Table 2, the fuel pretreatment method of the embodiment of the present application is used to pretreat the fuel, which reduces the average emission of nitrogen oxides in the flue gas and the concentration of nitrogen oxides in the flue gas.

[0168] (6) It can be seen from Table 3 that the fuel is pretreated by the fuel grading pretreatment method of the embodiment of the present application. The pretreated second fuel is used to supplement the heat of the upper material layer and reduce the ignition temperature. The particle size distribution makes the fuel burn more slowly and the heat release process is more gentle, avoiding the rapid dissipation of heat into the environment after concentrated release. The upper material layer can have sufficient heat supplement and insulation time to improve its mineralization conditions. In addition, under the effect of fuel surface addition, the maximum temperature difference of the material layers in each embodiment is 67°C (Example 5, the temperature difference between 700mm and 300mm) and the minimum is 32°C (Example 1, the temperature difference between 700mm and 300mm), while the maximum temperature difference of the material layer in Comparative Example 1 which does not adopt fuel surface addition is 169°C (Comparative Example 1, the temperature difference between 700mm and 100mm), indicating that fuel surface addition optimizes the temperature distribution of the sintering material layer. Combined with the carbon reduction measures, it not only reduces the sintering solid energy consumption, but also further reduces the temperature difference between the upper and lower parts of the sintering material layer, making the sintering temperature distribution of each part of the material layer more uniform during sintering, thereby ensuring that the upper material layer has suitable heat to improve the mineralization conditions, and the lower material layer avoids overburning caused by excess heat.

[0169] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A fuel classification pretreatment method, characterized in that: Includes steps: Formulating the solid fuel into a first fuel and a second fuel according to a particle size distribution; Performing a first pretreatment on the first fuel to obtain a first pretreated fuel; performing a second pretreatment on the second fuel to obtain a second pretreated fuel; The mass percentage of the particle size distribution of the first fuel includes: 10% to 35% for particle size ≥ 3mm, 50% to 65% for particle size 1mm≤<3mm, and 15% to 25% for particle size <1mm; The mass percentages of the particle size distribution of the second fuel include: 30% to 50% for a particle size ≥ 3 mm, 30% to 60% for a particle size 1 mm ≤ < 3 mm, and 10% to 20% for a particle size < 1 mm.

2. The fuel classification pretreatment method according to claim 1, characterized in that: The first pretreatment comprises the step of mixing the first fuel with lime milk.

3. The fuel classification pretreatment method according to claim 2, characterized in that: The mass ratio of the first fuel to the lime milk is 1:(1.5-2.5).

4. The fuel classification pretreatment method according to any one of claims 1 to 3, characterized in that: The second pretreatment comprises the steps of: mixing the second fuel with lime milk slurry; and the lime milk slurry components include lime milk and iron ore concentrate.

5. The fuel classification pretreatment method according to claim 4, characterized in that: The mass ratio of the second fuel to the lime milk slurry is (2-3):

1.

6. A sintering method, characterized in that: The steps include: Pretreating the solid fuel according to the pretreating method according to any one of claims 1 to 5 to obtain the first pretreating fuel and the second pretreating fuel; The first pretreated fuel and the raw material to be sintered are formed into a sintering material layer; After the second pretreated fuel is distributed on the sintering material layer to form a supplementary heat material layer, ignition and sintering are performed.

7. The sintering method according to claim 6, characterized in that: The mass ratio of the first fuel to the second fuel is: (90-96):(4-10); And / or, the height of the sintering material layer is greater than 900 mm.

8. The sintering method according to claim 6, characterized in that: The cloth processing comprises the steps of: The second pre-treated fuel is laid on a surface of the sintering material layer including a plurality of material grooves to form the supplementary heat material layer.

9. The sintering method according to claim 8, characterized in that: The depth of the material groove is less than 60 mm.

10. Use of the sintering method according to any one of claims 6 to 9 in the field of sintering of iron and steel metallurgy.