Method for preparing hematite pellets by using waste activated carbon
By mixing waste activated carbon powder with hematite and baking, the problem of unused value of waste activated carbon is solved, the strength and production efficiency of hematite pellets are improved, and solid waste recycling in the steel industry is realized. Cost reduction.
Patent Information
- Application Number
- CN202411218652.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-06
AI Technical Summary
The value of waste activated carbon generated by flue gas desulfurization and denitrification of steel enterprises has not been fully utilized and it is difficult to meet the requirements of blast furnace fuel.
After mixing waste activated carbon powder with hematite, the finely ground powder is made into balls in a disc pellet machine, and oxidation and roasting are carried out in a grate-rotating kiln to utilize the high specific surface area of waste activated carbon and combustion reactivity strengthens the consolidation of hematite pellets and reduces fuel demand.
The preheated ball strength and compressive strength of the finished ball pellets have been improved, the roasting is advanced, the amount of coal spraying at the rotary kiln head is reduced, the production cost is reduced, and the waste is harmless. Recycling.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron and steel metallurgy, and more specifically discloses a method for preparing hematite pellets by using waste activated carbon. Background Art
[0002] Steel is one of China's important industrial raw materials. The traditional long-process smelting process will produce a large amount of SO2 and NO X The sintering process produces SO2 and NO X The main source of SO2 and NO. Sintering pellet flue gas desulfurization and denitrification has become a hot topic in current research. Activated carbon has the ability to adsorb SO2 and NO at the same time. X , large specific surface area, high activity, stable chemical properties, low cost and other advantages, it has received widespread attention in the field of integrated desulfurization and denitrification of sintering flue gas. The desulfurization and denitrification device of the flue gas in the sintering pelletizing process uses an activated carbon flue gas purification device in the adsorption tower to purify the flue gas, which can comprehensively remove harmful substances such as sulfur dioxide, nitrogen oxides and dioxins in the flue gas, completely eliminate the corrosion of the surrounding environment by the emitted harmful substances, and can greatly reduce the emission of particulate matter. The activated carbon in the activated carbon flue gas purification device is added to the adsorption tower from the top of the tower, and moves downward under the action of gravity and the discharge device at the bottom of the tower. During the movement, small particles of waste activated carbon powder will fall out.
[0003] At present, the waste activated carbon produced by flue gas desulfurization and denitrification in steel enterprises is mainly used for blast furnace coal injection, but because the combustion value and combustible carbon of waste activated carbon powder are low, it is difficult to meet the requirements of blast furnace for fuel, and the value of waste activated carbon is not fully utilized. Therefore, the development of an energy-saving and environmentally friendly technology for efficient utilization of waste desulfurization and denitrification activated carbon is of great significance for steel plants to achieve harmless and recycled solid waste. Summary of the invention
[0004] The present invention mainly provides a method for preparing hematite pellets using waste activated carbon, which can solve the problem that the value of waste activated carbon produced by flue gas desulfurization and denitrification in steel enterprises is not fully utilized.
[0005] To solve the above technical problems, according to one aspect of the present invention, more specifically, a method for preparing hematite pellets using waste activated carbon comprises the following steps:
[0006] S1. Collecting waste activated carbon in the flue gas purification device and crushing the collected waste activated carbon;
[0007] S2, after the crushed waste activated carbon powder is mixed with the hematite, it enters the grinding system for grinding treatment, and the finely ground waste activated carbon powder and the hematite are dehydrated and precipitated, and then mixed with other pelletizing raw materials to obtain a mixture;
[0008] S3, pelletizing the above mixture in a disc pelletizing machine to obtain raw pellets containing activated carbon powder;
[0009] S4. The obtained green pellets containing activated carbon powder are sent to a chain grate-rotary kiln for oxidation roasting to obtain finished pellets.
[0010] Furthermore, in step S1, the calorific value of activated carbon powder is ≥28MJ / kg, the ignition point of activated carbon is 400-600℃, the fixed carbon content is ≥75%, the volatile matter is ≤10%, the ash content is ≤15%, and the moisture content is ≤8%. The ignition point of waste activated carbon is low. In the chain grate-rotary kiln process, the waste activated carbon mainly reacts in the second stage of preheating, which can increase the temperature of the preheating ball, realize the forward roasting, reduce the amount of coal injection at the kiln head of the rotary kiln, optimize the heat distribution of the rotary kiln, and improve the ring formation of the rotary kiln.
[0011] Furthermore, in step S1, the particle size of the fine-grained activated carbon powder is ≤1 mm, and the mass percentage content is more than 50%. This avoids the situation where the fuel particles are too coarse, the reaction is insufficient during the pellet preheating process, and sufficient secondary hematite cannot be generated to strengthen the Fe2O3 recrystallization consolidation, which is not conducive to improving the strength of the preheated balls.
[0012] Furthermore, in step S2, hematite accounts for ≥80% of the mass percentage of the iron ore, and the other iron ore is magnetite. After the hematite is treated by grinding, the surface activity of the hematite is increased, and it is difficult to dehydrate and settle. During the mixed sedimentation and filtration process of the waste activated carbon powder and the hematite, the waste activated carbon powder has rich micropores on the surface and can act as a carrier. Through the principle of carrier sedimentation, the sedimentation and filtration performance of the hematite is enhanced, the dehydration efficiency of the hematite is improved, and the energy consumption of sedimentation and filtration is reduced.
[0013] Furthermore, in step S2, the mass percentage of activated carbon powder in the mixture is 0.2%-0.8%.
[0014] Furthermore, in step S2, the mass percentage of the binder in the mixture is 0.6%-0.8%.
[0015] Furthermore, in step S2, the grinding treatment can be selected from one or more combinations of ball milling and high pressure roller milling, and the particles <0.073 mm in the mixed material after grinding treatment account for more than 80% of the total mass of the mixed material on a dry basis, and the specific surface area of the mixed material is >1500cm 2 / g.
[0016] Furthermore, in step S3, the moisture content of the pelletizing is 7.0-8.0%, the pelletizing time is 8-12 minutes, the diameter of the prepared raw pellets is 10-14 mm, and the ratio is ≥75%.
[0017] Furthermore, in step S4, a chain grate-rotary kiln process is adopted to prepare preheated balls with a compressive strength of 260-320 N / piece and a FeO content of 1.0-2.0%, and the prepared finished balls have a compressive strength of ≥2500 N / piece and a FeO content of ≤1%.
[0018] The beneficial effects of the method of using waste activated carbon to prepare hematite pellets of the present invention are:
[0019] (1) In view of the problem that waste activated carbon powder has low combustion value, low combustible carbon and poor strength, and cannot be used as blast furnace fuel, a method for strengthening the consolidation of hematite pellets by utilizing the characteristics of waste activated carbon with high specific surface area and fast combustion reaction is proposed, which can efficiently utilize the value of waste activated carbon and is conducive to the harmless and recycling of solid waste in the steel industry.
[0020] (2) In the chain grate-rotary kiln process, the reaction temperature of the traditional internal fuel is high, and it does not react or reacts little in the preheating section. The combustion is mainly concentrated at the kiln tail, resulting in local high temperature in the rotary kiln. In the high-proportion hematite pellets, the process of fine grinding of activated carbon powder is adopted to improve its combustion reactivity and reduce its ignition point, so that the activated carbon powder can fully react in the preheating section, promote the formation of secondary hematite to strengthen the recrystallization and consolidation of Fe2O3, improve the strength and temperature of the preheated balls, realize the forward roasting, reduce the amount of coal injection at the kiln head of the rotary kiln, avoid local high temperature in the rotary kiln, and improve the serious ringing problem of the rotary kiln in the preparation of high-proportion hematite pellets by the chain grate-rotary kiln.
[0021] (3) It can break through the limitation of pellet raw material resources, reduce pellet production cost, and have certain economic benefits. DETAILED DESCRIPTION
[0022] The present invention will be described in detail below in conjunction with embodiments. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other without conflict.
[0023] According to one aspect of the present invention, a method for preparing hematite pellets using waste activated carbon is provided. The chemical composition of the iron ore powder is shown in Table 1.
[0024] Table 1 Chemical composition of iron ore powder
[0025]
[0026]
[0027] Example
[0028] A: Collect the waste activated carbon in the flue gas purification device, crush and grind the waste activated carbon powder to obtain fine-grained activated carbon powder; the fine-grained activated carbon powder has a particle size of ≤1mm and a mass percentage of 65.88%. The activated carbon powder has a calorific value of 29.26MJ / kg, a fixed carbon content of 58.45%, a volatile content of 6.77%, an ash content of 11.50%, and a moisture content of 10.15%.
[0029] B: Mix the iron ore, fine-grained activated carbon powder and binder evenly, and grind them. After grinding, filter and settle, and the moisture content of the filter cake is 9.0%. The mass ratio of hematite A: hematite B: magnetite C in the iron ore is 35:45:20. The ratio of activated carbon powder, binder and iron ore is 0.2%, 0.6%:1. After the crushed waste activated carbon powder is mixed with hematite, it enters the grinding system for grinding treatment. After the finely ground waste activated carbon powder and hematite are dehydrated and settled, they are mixed with other ball-making raw materials to obtain a mixture.
[0030] C: The above mixture is pelletized in a disc pelletizer to obtain raw pellets containing activated carbon powder. The pelletizing time is 10 minutes and the moisture content of the pellets is controlled at 8.5%.
[0031] D: Send the green pellets containing activated carbon powder into the chain grate-rotary kiln for oxidation roasting. The chain grate preheating temperature is 730℃, the preheating temperature of the second stage is 1030℃, and the rotary kiln roasting temperature is 1250℃.
[0032] The compressive strength of the prepared preheated ball is 320N / piece, and the FeO content is 2.0%. The compressive strength of the prepared finished ball is 2600N / piece, and the FeO content is 0.8%.
[0033] Comparison Example
[0034] A: Mix the iron ore, coal powder and binder evenly, and perform wet ball milling. After grinding, filter and settle, and the filter cake has a moisture content of 10.0%. The mass ratio of hematite A: hematite B: magnetite C in the iron ore is 35:45:20. The ratio of coal powder, binder and iron ore is 0.5%, 0.6%:1.
[0035] B: The above mixture is pelletized in a disc pelletizer to obtain raw pellets containing activated carbon powder. The pelletizing time is 10 minutes and the moisture content of the pellets is controlled at 8.5%.
[0036] C: Send the green pellets containing activated carbon powder into the chain grate-rotary kiln for oxidation roasting. The chain grate preheating temperature is 730℃, the second preheating temperature is 1030℃, and the rotary kiln roasting temperature is 1250℃.
[0037] The compressive strength of the prepared preheated ball is 260N / piece, and the FeO content is 1.6%. The compressive strength of the prepared finished ball is 2530N / piece, and the FeO content is 1.0%.
[0038] Compared with the control example, the pellet raw materials are filtered and settled after grinding, the moisture content of the filter cake is reduced, and the compressive strength of the prepared preheated balls and finished balls is greatly improved.
[0039] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by ordinary technicians in this technical field within the essential scope of the present invention also fall within the protection scope of the present invention.
Claims
1. A method for preparing hematite pellets using waste activated carbon, characterized in that: The following steps are involved: S1. Collecting waste activated carbon in the flue gas purification device and crushing the collected waste activated carbon; S2, after the crushed waste activated carbon powder is mixed with the hematite, it enters the grinding system for grinding treatment, and the finely ground waste activated carbon powder and the hematite are dehydrated and precipitated, and then mixed with other pelletizing raw materials to obtain a mixture; S3, pelletizing the above-mentioned mixture in a disc pelletizing machine to obtain raw balls containing activated carbon powder; S4. The obtained green pellets containing activated carbon powder are sent to a chain grate-rotary kiln for oxidation roasting to obtain finished pellets.
2. The method for preparing hematite pellets using waste activated carbon according to claim 1, characterized in that: In the step S1, the calorific value of the activated carbon powder is ≥28 MJ / kg, the ignition point of the activated carbon is 400-600°C, the fixed carbon content is ≥75%, the volatile matter is ≤10%, the ash content is ≤15%, and the moisture content is ≤8%.
3. The method for preparing hematite pellets using waste activated carbon according to claim 1, characterized in that: In the step S1, the particle size of the fine-grained activated carbon powder is ≤1 mm, and the mass percentage content is more than 50%.
4. The method for preparing hematite pellets using waste activated carbon according to claim 1, characterized in that: In step S2, the mass percentage of hematite in the iron ore is ≥80%, and the rest of the iron ore is magnetite.
5. The method for preparing hematite pellets using waste activated carbon according to claim 1, characterized in that: In step S2, the mass percentage of activated carbon powder in the mixed material is 0.2%-0.8%.
6. The method for preparing hematite pellets using waste activated carbon according to claim 1, characterized in that: In step S2, the mass percentage of the binder in the mixture is 0.6%-0.8%.
7. The method for preparing hematite pellets using waste activated carbon according to claim 1, characterized in that: In step S2, the grinding treatment can be selected from one or more combinations of ball milling and high pressure roller milling. In the mixture treated with grinding, particles <0.073 mm account for more than 80% of the total mass of the dry basis of the mixture, and the specific surface area of the mixture is >1500cm 2 / g.
8. The method for preparing hematite pellets using waste activated carbon according to claim 1, characterized in that: In the step S3, the moisture content of the pelletizing is 7.0-8.0%, the pelletizing time is 8-12 minutes, the diameter of the prepared green pellets is 10-14 mm, and the ratio is ≥75%.
9. The method for preparing hematite pellets using waste activated carbon according to claim 1, characterized in that: In the step S4, a chain grate-rotary kiln process is adopted to prepare preheated balls with a compressive strength of 260-320 N / piece and a FeO content of 1.0-2.0%. The prepared finished balls have a compressive strength of ≥2500 N / piece and a FeO content of ≤1%.