Copper anode slime treatment process
Through the process of high-pressure oxidation leaching, barium sulfate transformation and barium separation, the long treatment cycle and high energy consumption caused by the high content of barium sulfate in copper anode mud are solved, and the efficient treatment of copper anode mud and the effective precious metals are achieved. Recycle.
Patent Information
- Application Number
- CN202411297570.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-12-06
AI Technical Summary
During the ignition smelting process of copper anode mud, the presence of barium sulfate leads to a long treatment cycle, high energy consumption, and it is difficult to avoid the separation of lead, affecting the enrichment efficiency of precious metals.
Using high-pressure oxidation leaching, barium sulfate transformation and barium separation process flow, high-pressure oxidation leaching removes copper and some impurities, barium sulfate transformation reduces barium content, and hydrochloric acid separates barium and bismuth to avoid the separation of lead and improves the enrichment of precious metals. efficiency.
It effectively reduces the barium content in copper anode mud, shortens the ignition smelting time and temperature, improves the processing capacity, reduces energy consumption, and retains lead to capture precious metals, and improves the recovery rate of gold and silver.
Smart Images

Figure CN119082466A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of precious metal lifting, in particular to a copper anode mud treatment process. Background Art
[0002] In a copper smelter, while anode copper is electrolytically refined to obtain cathode copper, copper anode mud is also produced. Copper anode mud is an important source for extracting precious metals. Copper anode mud is rich in rare and precious metals such as gold, silver, platinum, palladium, selenium, tellurium, as well as metals such as copper, lead and barium.
[0003] At present, the treatment of copper anode mud mostly adopts pyrometallurgical process. The pyrometallurgical process of copper anode mud has the advantages of large processing capacity and simple equipment operation, and is mostly adopted by copper smelting enterprises with large production scale. The pyrometallurgical process of copper anode mud treatment by Kaldo furnace has gradually become the main treatment process of copper anode mud with its own technical and environmental advantages.
[0004] The process flow of the Kaldo furnace process for treating copper anode mud is as follows: copper anode mud is leached with high-pressure oxygen to obtain decopperized anode mud. After drying, the decopperized anode mud is added to the Kaldo furnace together with the solvent for smelting. The smelting is divided into two stages: Kaldo furnace smelting: the physical in the Kaldo furnace is heated and melted. Under the action of the solvent, precious metals such as gold, silver, platinum and palladium are enriched in the lead, and the upper smelting slag is separated to form a lead alloy. Kaldo furnace blowing: oxygen is blown into the lead alloy to oxidize and volatilize the lead to form a doer alloy. Then it is cast into a doer alloy plate for silver electrolysis to obtain silver and silver anode mud. The silver anode mud is further refined to recover gold and produce platinum-palladium concentrate as a raw material for recovering platinum and palladium.
[0005] Copper anode mud is the product of copper electrolysis. The copper electrolysis process requires copper anode plates. When producing copper anode plates, in order to improve the demoulding effect of copper anode plates, it is necessary to spray barium sulfate solution on the casting mold. The barium sulfate solution is inevitably entrained on the copper anode plate. Although the copper anode plate is cleaned before entering the electrolytic cell, it cannot be completely cleaned. It is eventually enriched in the copper anode mud, and the content in the copper anode mud is generally high, generally 15-20%. This correspondingly reduces the content of gold and silver. When smelting copper anode mud, it is necessary to add materials in batches for smelting, which makes the operation cycle long. In addition, the melting point of barium sulfate is relatively high, reaching 1580℃. In order to melt copper anode mud, the temperature in the furnace needs to be increased accordingly; thus, due to the presence of barium sulfate, the smelting operation cycle of copper anode mud is long and the smelting temperature is high, thereby increasing energy consumption and reducing the service life of the Kaldo furnace.
[0006] In order to reduce the content of barium sulfate in copper anode mud, CN207828384U discloses a separation device for barium sulfate in copper anode mud, CN206858624U discloses an efficient enrichment and separation device for barium sulfate in anode mud, and uses physical methods to separate barium sulfate in copper anode mud, thereby reducing the content of barium sulfate in copper anode mud. However, this method of separating barium sulfate causes a certain amount of valuable metals such as gold and silver to enter the barium sulfate, and it is necessary to further recover the valuable metals such as gold and silver in the barium sulfate. CN114807599 A is a process suitable for treating barium sulfate slag in copper anode mud, which is a treatment method for barium sulfate separated by the above method, so as to further recover valuable metals such as gold and silver in the barium sulfate. CN112609078B is a copper anode mud treatment process, which adopts three process stages: (1) anode mud wet removal of copper, selenium and tellurium stage; (2) anode mud wet removal of lead, barium and bismuth stage; (3) Kaldor furnace smelting stage. This patent uses anode mud to remove all copper, part of selenium and tellurium in the first process stage to produce corresponding copper, tellurium and selenium products; the second process stage removes all lead, barium and bismuth to produce corresponding lead, barium and bismuth products; the first two process stages pre-treatment and impurity removal provide a new anode mud Kaldo furnace smelting treatment idea. However, this method, in the second stage, separates lead and bismuth at the same time as separating barium, and Kaldo slag needs to use lead and bismuth to capture precious metals such as gold, silver, platinum and palladium during the smelting stage. Sometimes, metal lead is added to the copper anode mud during production to increase the amount of lead and increase the enrichment of gold and silver. Summary of the invention
[0007] The purpose of the embodiments of the present application is to provide a copper anode mud treatment process, which is used to avoid the separation of lead when separating barium from copper anode mud, meet the demand for lead capture of precious metals during pyrometallurgy, and reduce the long pyrometallurgy treatment cycle and high energy consumption of copper anode mud.
[0008] To achieve the above objectives, the present application provides the following technical solutions: A copper anode mud treatment process comprises the following steps: 1) High-pressure oxidation leaching of copper anode mud, filtering to obtain decopperized anode mud and primary filtrate; 2) Add ammonium carbonate to the copper-removed anode mud for barium sulfate transformation to obtain transformed copper-removed anode mud and secondary filtrate; 3) Adding hydrochloric acid to the copper-removing anode mud to separate barium and bismuth, filtering to obtain copper-removing barium anode mud and tertiary filtrate; 4) De-copperize barium anode mud smelting to obtain precious metal alloys.
[0009] Furthermore, the copper anode mud includes: 0.1wt% to 0.8wt% Au; 2.5wt% to 10wt% Ag; 1.5wt% to 6wt% Se; 6wt% to 13wt% Cu; 1wt% to 5wt% As; 0.2wt% to 1.2wt% Sb; 20wt% to 40wt% Pb; 0.2wt% to 1.5wt% Te; 2wt% to 10wt% Bi; 10wt% to 25wt% Ba; the remainder is other metals and impurities.
[0010] Furthermore, the process conditions of the high-pressure oxidation leaching in step 1) are: sulfuric acid concentration of 150-300 g / L, liquid-to-solid ratio of 3-6:1, temperature of 135°C-180°C, time of 2-6 h, and pressure of 0.4-0.75 MPa.
[0011] Furthermore, the copper-removed anode mud in step 2) is transformed into barium sulfate by adding ammonium carbonate, specifically: The decopperized anode mud is added into water for slurrying to obtain decopperized anode mud slurry, and then ammonia water is added to adjust the pH of the decopperized anode mud slurry to 6-8; Then, an ammonium carbonate solution is added to the decopperized anode slurry to carry out a transformation reaction.
[0012] Furthermore, the slurrying process conditions are: liquid-solid ratio of 7 to 10:1; the transformation reaction conditions are: ammonium carbonate concentration of 2 to 5 mol / L, reaction temperature of 80°C to 90°C, and reaction time of 3 to 4 hours.
[0013] Further, the step of adding hydrochloric acid to separate barium and bismuth in step 3) is: The transformation decopperized anode mud is added into water for slurrying, with a liquid-to-solid ratio of 2 to 5:1, to obtain transformation decopperized anode mud slurry; Then, hydrochloric acid is added to the transformation decopperized anode slurry to carry out leaching reaction. The leaching reaction conditions are: hydrochloric acid concentration of 1-3 mol / L, reaction temperature of 50°C-90°C, and reaction time of 2-5 hours.
[0014] Furthermore, the tertiary filtrate is mixed with the secondary filtrate to react, and the barium sulfate and bismuth oxychloride solutions are obtained by filtration; the bismuth oxychloride solution is hydrolyzed and precipitated, and the bismuth oxychloride and ammonium carbonate solutions are obtained by filtration.
[0015] Further, the step of pyrometallurgical smelting of the copper-removed barium anode mud in step 4) is: Sodium carbonate, quartz stone, coke powder and the copper-free barium anode mud are mixed, smelted and blown to obtain a precious metal alloy.
[0016] Furthermore, the sodium carbonate, the quartz stone, the coke powder and the decoppered barium anode mud are mixed in a mass ratio of (3-7):(3-6):(3-5):100, the smelting temperature is 880-920° C., and the smelting time is 2-4 hours.
[0017] Furthermore, the blowing includes primary blowing and secondary blowing; The oxygen enrichment flow rate of the primary blowing is 500~700 Nm 3 / h, oxygen volume concentration is 20~22%, furnace speed is 10~12 r / min, melt temperature in the furnace is 1150~1200℃, and blowing time is 4~5h; The oxygen enrichment flow rate of the secondary blowing is 600~750 Nm 3 / h, oxygen volume concentration is 25~35%, furnace speed is 15~16 r / min, melt temperature in the furnace is 1200~1250℃, and blowing time is 2~3h.
[0018] Compared with the prior art, the beneficial effects of this application are: 1) Through barium sulfate transformation, about 20% of barium and about 3% of bismuth in the copper-removed anode mud are separated, so that the mass of the copper-removed barium anode mud is reduced by about 23% relative to the copper-removed anode mud.
[0019] 2) With the same Kaldo furnace material loading, the copper anode mud processing capacity is relatively increased by 23%.
[0020] 3) Due to the removal of barium, the melting and smelting difficulty of the copper-removed barium anode mud is reduced, the smelting temperature is reduced by at least 20°C, and the smelting time is reduced by at least 30 minutes, which correspondingly reduces the energy consumption of Kaldo furnace smelting. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the process flow chart for this application. DETAILED DESCRIPTION
[0022] The present application provides a copper anode slime treatment process, comprising the following steps: 1) High-pressure oxidation leaching of copper anode mud, filtering to obtain decopperized anode mud and primary filtrate; 2) Add ammonium carbonate to the copper-removed anode mud for barium sulfate transformation to obtain transformed copper-removed anode mud and secondary filtrate; 3) Adding hydrochloric acid to the copper-removing anode mud to separate barium and bismuth, filtering to obtain copper-removing barium anode mud and tertiary filtrate; 4) De-copperize barium anode mud smelting to obtain precious metal alloys.
[0023] The preferred composition of the copper anode mud treated in the present application is: 0.1wt% to 0.8wt% Au; 2.5wt% to 10wt% Ag; 1.5wt% to 6wt% Se; 6wt% to 13wt% Cu; 1wt% to 5wt% As; 20wt% to 40wt% Pb; 0.2wt% to 1.5wt% Te; 2wt% to 10wt% Bi; 10wt% to 25wt% Ba; the remainder is other metals and impurities.
[0024] More preferably, the composition of the copper anode mud is: 0.15wt%~0.3wt% Au; 3wt%~6wt% Ag; 2wt%~4.5wt% Se; 8wt%~12wt% Cu; 1.5wt%~3wt% As; 30wt%~40wt% Pb; 0.5wt%~1wt% Te; 3wt%~7wt% Bi; 15wt%~20wt% Ba; the balance is other metals and impurities.
[0025] Barium sulfate is a mold release agent added during the casting of copper anode plates. Due to the stability of barium sulfate, it does not react during the electrolysis process, so the barium entering the copper anode mud still exists in the form of barium sulfate, that is, the barium in the copper anode mud described in this application exists in the form of barium sulfate.
[0026] The process of high-pressure oxidation leaching described in the present application is: first, a dilute sulfuric acid solution is prepared in an autoclave according to a sulfuric acid concentration of 150 to 300 g / L, and then the copper anode mud is added to the autoclave and mixed with the dilute sulfuric acid solution according to a liquid-solid ratio of 3 to 6:1. Then, the mixed slurry in the autoclave is heated, generally using steam, and after the temperature reaches 135°C to 180°C, high-pressure oxygen is introduced, and the pressure in the autoclave reaches 0.4 to 0.75 MPa through the introduction of high-pressure oxygen, and a high-pressure oxidation leaching reaction is carried out, and the reaction time is controlled at 2 to 6 hours.
[0027] The preferred process conditions for high-pressure oxidation leaching are: liquid-to-solid ratio 4-5:1, sulfuric acid concentration 200-300 g / L, reaction temperature 160°C-170°C, reaction pressure 0.6-0.7 MPa, and reaction time 4-5 h.
[0028] The main purpose of high-pressure oxidation leaching is to remove copper from anode mud. Some of the copper in copper anode mud exists in the form of single copper particles, which need to be oxidized into divalent copper ions that are easily soluble in sulfuric acid solution. In order to increase the oxidation rate of copper, that is, to increase the dissolution rate of copper, high pressure is used to increase the oxidation process of copper under the condition of oxygen. While copper is oxidized, some other impurity elements such as silver, selenium, tellurium, etc. will also be oxidized into ions that are easily soluble in sulfuric acid solution. Therefore, high-pressure oxidation leaching transfers most of the copper in anode mud, as well as some impurities such as silver, selenium, tellurium and arsenic from the slag phase to the liquid phase.
[0029] After high-pressure oxidation leaching is completed, the slurry is pumped to the filter press for solid-liquid separation, and the copper-free anode mud and the primary filtrate are obtained after separation. The primary filtrate is further used to recover valuable metals such as silver, selenium, and tellurium.
[0030] Since barium sulfate has good stability and does not react in the sulfuric acid system, the barium in the copper-removed anode mud still exists in the form of barium sulfate after the high-pressure oxidation leaching. Therefore, in the prior art, after the high-pressure oxidation copper removal, the smelting and blowing processes, especially the smelting process, have the problems of high smelting temperature and long smelting time.
[0031] The copper-removed anode mud in this application is added with ammonium carbonate to transform into barium sulfate, and the specific steps are: The decopperized anode mud is added into water for slurrying at a liquid-solid ratio of 7 to 10:1 to obtain decopperized anode mud slurry, and then ammonia water is added to adjust the pH of the decopperized anode mud slurry to 6 to 8.
[0032] Then, an ammonium carbonate solution is added to the copper-removed anode slurry at an ammonium carbonate concentration of 2 to 5 mol / L to perform a transformation reaction at a temperature of 80° C. to 90° C. and a reaction time of 3 to 4 hours.
[0033] After the transformation reaction is completed, filtration is performed to obtain the transformation decoppered anode mud and secondary filtrate.
[0034] In order to reduce the consumption of ammonia water in the present application, the decopperized anode mud is generally washed with water before being slurried to remove sulfuric acid in the decopperized anode.
[0035] The principle of barium sulfate transformation is that the solubility of barium carbonate is lower than that of barium sulfate. In a high-concentration carbonate system and high temperature conditions, barium sulfate can be converted into barium carbonate. The main reaction formula is:
[0036] The step of adding hydrochloric acid to separate barium and bismuth in step 3) of the present application is: The transformation decoppering anode mud is added into water for slurrying, and the liquid-to-solid ratio is 2-5:1 to obtain the transformation decoppering anode mud slurry.
[0037] Then, hydrochloric acid is added to the transformation decopperized anode slurry to carry out leaching reaction. The leaching reaction conditions are: hydrochloric acid concentration of 1-3 mol / L, reaction temperature of 50°C-90°C, and reaction time of 2-5 hours.
[0038] After the leaching reaction is completed, the copper-removed barium anode mud and the tertiary filtrate are obtained by filtration.
[0039] In this step, the reaction between hydrochloric acid and barium carbonate is used to form barium chloride which is easily soluble in water, so that the barium in the transformation decoppering anode mud enters the solution. The bismuth in the transformation decoppering anode mud is also converted into bismuth oxychloride under the action of hydrochloric acid and enters the solution like barium chloride. The lead in the transformation decoppering anode mud will exist in the form of lead sulfate and lead chloride, which are basically insoluble in the hydrochloric acid system, thereby achieving the purpose of separating barium from other metals.
[0040]
[0041] In order to further separate the barium and utilize the intermediate material, in the present application, the secondary filtrate is mixed with the tertiary filtrate to react, and the sulfate in the secondary filtrate is reacted with the barium ions in the tertiary filtrate to form a barium sulfate precipitate, which is filtered to obtain a barium sulfate and bismuth oxychloride solution. The bismuth oxychloride solution is further hydrolyzed and precipitated, and bismuth oxychloride and ammonium carbonate solution are obtained by filtration, and the ammonium carbonate solution is returned to step 2) the barium sulfate transformation step.
[0042] The decoppered barium anode mud pyrometallurgical smelting step described in step 4) of this application is: Sodium carbonate, quartz stone, coke powder and the copper-free barium anode mud are mixed, smelted and blown to obtain a precious metal alloy.
[0043] The sodium carbonate, quartz stone, coke powder and decoppered barium anode mud are mixed in a mass ratio of (3-7): (3-6): (3-5): 100 and then smelted at a smelting temperature of 880-920° C. for 2-3 hours.
[0044] After the smelting is completed, the first and second blowing processes are carried out.
[0045] The oxygen-enriched flow rate of the primary blowing is 500-700 Nm3 / h, the oxygen volume concentration is 20-22%, the furnace speed is 10-12 r / min, the melt temperature in the furnace is 1150-1200°C, and the blowing time is 4-5h.
[0046] The oxygen-enriched flow rate of the secondary blowing is 600-750 Nm3 / h, the oxygen volume concentration is 25-35%, the furnace speed is 15-16 r / min, the melt temperature in the furnace is 1200-1250°C, and the blowing time is 2-3h.
[0047] After blowing, precious metal alloy is obtained, silver is recovered from the precious metal alloy through silver electrolysis process, and gold is obtained from silver anode mud through gold refining process.
[0048] From the above, the copper anode mud treatment process provided by the present application adopts a process of removing barium sulfate before smelting, and retains lead for capturing precious metals such as gold and silver, so that the present application has a detailed improvement in the copper anode mud treatment, as follows: 1) Through barium sulfate transformation, about 20% of barium and about 3% of bismuth in the copper-removed anode mud are separated, so that the mass of the copper-removed barium anode mud is reduced by about 23% relative to the copper-removed anode mud.
[0049] 2) With the same Kaldo furnace material loading, the copper anode mud processing capacity is relatively increased by 23%.
[0050] 3) Due to the removal of barium, the melting and smelting difficulty of the copper-free barium anode mud is reduced, the smelting temperature is reduced by 20°C, and the smelting time is reduced by 30 minutes, which correspondingly reduces the energy consumption of the Kaldo furnace smelting.
[0051] In order to further illustrate the technical solution of the present application, the preferred implementation scheme of the present application is described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present application, rather than limiting the claims of the present application. Example
[0052] The composition of copper anode mud is as follows:
[0053] 1) High pressure oxidation leaching The high-pressure oxidation leaching conditions are liquid-to-solid ratio 4:1, sulfuric acid concentration 280g / L, reaction temperature 175℃, reaction pressure 0.5Mpa, and reaction time 5h.
[0054] The composition of the copper-removed anode mud is as follows:
[0055] 2) Barium sulfate transformation The process conditions for the barium sulfate transformation are: adding the decopperized anode mud into water for slurrying at a liquid-solid ratio of 10:1, and then adding ammonia water to adjust the pH of the decopperized anode mud slurry to 7.
[0056] Then, an ammonium carbonate solution is added to the decopperized anode slurry at an ammonium carbonate concentration of 5 mol / L to perform a transformation reaction at a temperature of 90° C. and a reaction time of 4 hours.
[0057] After the transformation reaction is completed, filtration is performed to obtain the transformation decoppered anode mud and secondary filtrate.
[0058] 3) Separation of barium and bismuth using hydrochloric acid The transformation decoppering anode mud is added into water for slurrying, and the liquid-to-solid ratio is 5:1, so as to obtain the transformation decoppering anode mud slurry.
[0059] Then, hydrochloric acid is added to the transformation decopperized anode slurry to carry out leaching reaction. The leaching reaction conditions are: hydrochloric acid concentration of 3 mol / L, reaction temperature of 90° C., and reaction time of 5 hours.
[0060] After the reaction, the copper-free barium anode mud and the tertiary filtrate are obtained by filtration; The composition of the copper-removed barium anode mud is as follows:
[0061] 4) Decopperized barium anode mud pyrometallurgy The sodium carbonate, quartz stone, coke powder and decoppered barium anode mud are mixed in a mass ratio of 7:3:5:100 and then smelted at a smelting temperature of 920° C. for 3 hours.
[0062] After the smelting is completed, the oxygen-enriched flow rate of the first blowing is 500Nm 3 / h, the oxygen volume concentration is 22%, the furnace speed is 12 r / min, the melt temperature in the furnace is 1160℃, and the blowing time is 5h.
[0063] The oxygen enrichment flow rate for secondary blowing is 730 Nm 3 / h, the oxygen volume concentration is 28%, the furnace speed is 15 r / min, the melt temperature in the furnace is 1220℃, and the blowing time is 2h.
[0064] After the blowing, a precious metal alloy is obtained, which contains 9.82% gold and 84.48% silver, with a gold recovery rate higher than 99.6% and a silver recovery rate higher than 99.2%. Example
[0065] The composition of copper anode mud is as follows:
[0066] 1) High pressure oxidation leaching The high-pressure oxidation leaching conditions are liquid-to-solid ratio 6:1, sulfuric acid concentration 180g / L, reaction temperature 175℃, reaction pressure 0.65Mpa, and reaction time 4h.
[0067] The composition of the copper-removed anode mud is as follows:
[0068] 2) Barium sulfate transformation The process conditions for the barium sulfate transformation are: adding the decopperized anode mud into water for slurrying at a liquid-solid ratio of 7:1, and then adding ammonia water to adjust the pH of the decopperized anode mud slurry to 8.
[0069] Then, an ammonium carbonate solution is added to the decopperized anode slurry at an ammonium carbonate concentration of 2 mol / L to perform a transformation reaction at a temperature of 90° C. and a reaction time of 4 hours.
[0070] After the transformation reaction is completed, filtration is performed to obtain the transformation decoppered anode mud and secondary filtrate.
[0071] 3) Separation of barium and bismuth using hydrochloric acid The transformation decoppering anode mud is added into water for slurrying, and the liquid-to-solid ratio is 3:1, so as to obtain the transformation decoppering anode mud slurry.
[0072] Then, hydrochloric acid is added to the transformation decopperized anode slurry to carry out leaching reaction. The leaching reaction conditions are: hydrochloric acid concentration of 1.5 mol / L, reaction temperature of 80° C., and reaction time of 2.5 hours.
[0073] After the reaction, the copper-free barium anode mud and the tertiary filtrate are obtained by filtration; The composition of the copper-removed barium anode mud is as follows:
[0074] 4) De-coppering barium anode mud pyrometallurgy The sodium carbonate, quartz stone, coke powder and decoppered barium anode mud are mixed in a mass ratio of 3:5:4:100 and then smelted at a smelting temperature of 890° C. for 3 hours.
[0075] After the smelting is completed, the oxygen-enriched flow rate of the first blowing is 700Nm 3 / h, the oxygen volume concentration is 20%, the furnace speed is 10 r / min, the melt temperature in the furnace is 1190℃, and the blowing time is 4h.
[0076] The oxygen enrichment flow rate for secondary blowing is 650 Nm 3 / h, the oxygen volume concentration is 32%, the furnace speed is 15 r / min, the melt temperature in the furnace is 1250℃, and the blowing time is 2h.
[0077] After the blowing, a precious metal alloy is obtained, which contains 10.72% gold and 87.28% silver, with a gold recovery rate higher than 99.7% and a silver recovery rate higher than 99.4%. Example
[0078] The composition of copper anode mud is as follows:
[0079] 1) High pressure oxidation leaching The high-pressure oxidation leaching conditions are liquid-to-solid ratio 3:1, sulfuric acid concentration 250g / L, reaction temperature 140°C, reaction pressure 0.75Mpa, and reaction time 6h.
[0080] The composition of the copper-removed anode mud is as follows:
[0081] 2) Barium sulfate transformation The process conditions for the barium sulfate transformation are: adding the decopperized anode mud into water for slurrying at a liquid-solid ratio of 9:1, and then adding ammonia water to adjust the pH of the decopperized anode mud slurry to 6.
[0082] Then, an ammonium carbonate solution is added to the decopperized anode slurry at an ammonium carbonate concentration of 4 mol / L to perform a transformation reaction at a temperature of 80° C. and a reaction time of 4 hours.
[0083] After the transformation reaction is completed, filtration is performed to obtain the transformation copper-removing anode mud and secondary filtrate.
[0084] 3) Separation of barium and bismuth using hydrochloric acid The transformation decoppering anode mud is added into water for slurrying, and the liquid-to-solid ratio is 5:1, so as to obtain the transformation decoppering anode mud slurry.
[0085] Then, hydrochloric acid is added to the transformation decopperized anode slurry to carry out leaching reaction. The leaching reaction conditions are: hydrochloric acid concentration is 2 mol / L, reaction temperature is 60° C., and reaction time is 4 hours.
[0086] After the reaction, the copper-free barium anode mud and the tertiary filtrate are obtained by filtration; The composition of the copper-removed barium anode mud is as follows:
[0087] 4) Decopperized barium anode mud pyrometallurgy The sodium carbonate, quartz stone, coke powder and decoppered barium anode mud are mixed in a mass ratio of 6:4:4:100 and then smelted at a temperature of 900° C. for 3 hours.
[0088] After the smelting is completed, the oxygen-enriched flow rate of the first blowing is 550Nm 3 / h, oxygen volume concentration is 22%, furnace speed is 10 r / min, melt temperature in the furnace is 1150℃, and blowing time is 5h.
[0089] The oxygen enrichment flow rate for secondary blowing is 700 Nm 3 / h, the oxygen volume concentration is 27%, the furnace speed is 16r / min, the melt temperature in the furnace is 1220℃, and the blowing time is 3h.
[0090] After the blowing, a precious metal alloy is obtained, which contains 10.02% gold and 87.78% silver, with a gold recovery rate higher than 99.6% and a silver recovery rate higher than 99.3%.
[0091] Although the present application has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A copper anode mud treatment process, comprising the following steps: 1) High-pressure oxidation leaching of copper anode mud, filtering to obtain decopperized anode mud and primary filtrate; 2) Add ammonium carbonate to the copper-removed anode mud for barium sulfate transformation to obtain transformed copper-removed anode mud and secondary filtrate; 3) Adding hydrochloric acid to the copper-removing anode mud to separate barium and bismuth, filtering to obtain copper-removing barium anode mud and tertiary filtrate; 4) De-copperize barium anode mud smelting to obtain precious metal alloys.
2. The copper anode mud treatment process according to claim 1, characterized in that: The copper anode mud includes: 0.1wt% to 0.8wt% Au; 2.5wt% to 10wt% Ag; 1.5wt% to 6wt% Se; 6wt% to 13wt% Cu; 1wt% to 5wt% As; 0.2wt% to 1.2wt% Sb; 20wt% to 40wt% Pb; 0.2wt% to 1.5wt% Te; 2wt% to 10wt% Bi; 10wt% to 25wt% Ba; the remainder is other metals and impurities.
3. The copper anode mud treatment process according to claim 1, characterized in that: The process conditions of high-pressure oxidation leaching in step 1) are: sulfuric acid concentration of 150-300 g / L, liquid-to-solid ratio of 3-6:1, temperature of 135°C-180°C, time of 2-6 h, and pressure of 0.4-0.75 MPa.
4. The copper anode mud treatment process according to claim 1, characterized in that: In step 2), the copper-removed anode mud is transformed into barium sulfate by adding ammonium carbonate, and the specific steps are: The decopperized anode mud is added into water for slurrying to obtain decopperized anode mud slurry, and then ammonia water is added to adjust the pH of the decopperized anode mud slurry to 6-8; Then, an ammonium carbonate solution is added to the decopperized anode slurry to carry out a transformation reaction.
5. The copper anode mud treatment process according to claim 4, characterized in that: The slurrying process conditions are: liquid-to-solid ratio of 7 to 10:1; the transformation reaction conditions are: ammonium carbonate concentration of 2 to 5 mol / L, reaction temperature of 80°C to 90°C, and reaction time of 3 to 4 hours.
6. The copper anode mud treatment process according to claim 1, characterized in that: The step of adding hydrochloric acid to separate barium and bismuth in step 3) is: The transformation decopperized anode mud is added into water for slurrying, with a liquid-to-solid ratio of 2 to 5:1, to obtain transformation decopperized anode mud slurry; Then, hydrochloric acid is added to the transformation decopperized anode slurry to carry out leaching reaction. The leaching reaction conditions are: hydrochloric acid concentration of 1-3 mol / L, reaction temperature of 50°C-90°C, and reaction time of 2-5 hours.
7. The copper anode mud treatment process according to claim 1, characterized in that: The tertiary filtrate is mixed with the secondary filtrate to react, and filtered to obtain a barium sulfate and bismuth oxychloride solution; the bismuth oxychloride solution is hydrolyzed and precipitated, and filtered to obtain a bismuth oxychloride and ammonium carbonate solution.
8. The copper anode mud treatment process according to claim 1, characterized in that: The steps of pyrometallurgical smelting of the copper-removed barium anode mud in step 4) are: Sodium carbonate, quartz stone, coke powder and the copper-free barium anode mud are mixed, smelted and blown to obtain a precious metal alloy.
9. The copper anode mud treatment process according to claim 8, characterized in that: The sodium carbonate, the quartz stone, the coke powder and the decoppered barium anode mud are mixed in a mass ratio of (3-7):(3-6):(3-5):100, the smelting temperature is 880-920° C., and the smelting time is 2-4 hours.
10. The copper anode mud treatment process according to claim 8, characterized in that: The blowing includes primary blowing and secondary blowing; The oxygen enrichment flow rate of the primary blowing is 500~700 Nm 3 / h, oxygen volume concentration is 20~22%, furnace speed is 10~12r / min, melt temperature in the furnace is 1150~1200℃, and blowing time is 4~5h; The oxygen enrichment flow rate of the secondary blowing is 600~750 Nm 3 / h, oxygen volume concentration is 25~35%, furnace speed is 15~16r / min, melt temperature in the furnace is 1200~1250℃, and blowing time is 2~3h.
Citation Information
Cited By
A method for treating high-nickel copper anode sludge
CN123084109A